◆ Rebuild

Part 8 · Chemistry

Activated Charcoal

Ordinary charcoal heated again to bright orange in steam — or charred after soaking in a strong salt or acid — becomes a sponge of microscopic pores, a teaspoon of which has an inner surface of a few thousand square metres, roughly the size of a football pitch. It pulls tastes, smells, colours and many poisons out of water, syrup, spirits and air, and out of a poisoned person's gut.

Difficulty
●●●●●
Time
One day to make the charcoal; two to four hours per activation run; an afternoon to grind, wash and size
Steps from zero
2 prerequisites →

You need first

Charcoal

This unlocks

—
The full path from nothing — 2 steps before this one
  1. Fire
  2. Charcoal
  3. Activated Charcoal

Do them roughly in this order. See it on the tech tree →

Why it matters

Charcoal does a little cleaning on its own: water poured through a bed of crushed charcoal tastes sweeter, and a pinch of charcoal dust on a smelly wound dressing takes away some of the stench. Activated charcoal does the same thing ten to a hundred times more strongly. With it you can:

  • take bad tastes, smells and colours out of drinking water — from peat, rotting leaves, swamp gas, oil, chlorine — in a simple filter (Finding and Purifying Water, Water Treatment for a Town);
  • whiten sugar syrup and other foods and medicines (Sugar, Making Medicines);
  • clean up spirits distilled for drinking, removing harsh-tasting oils (Distillation);
  • save poisoned people: swallowed soon enough, it soaks up many plant poisons and overdoses of medicine before they enter the blood (Dangerous Plants and Animals, Emergencies);
  • filter air in a respirator against solvent and tar fumes in the workshop;
  • purify chemicals in the laboratory, by stirring a pinch into a coloured solution before crystallising it (Identifying Substances).

All of it from wood, nutshells or bones and a hot fire.

How it works

Some substances stick to surfaces — not soaking into a material the way water soaks into a sponge (absorption), but clinging to its surface in a layer one molecule thick. This is adsorption (with a d). Carbon is especially good at it for oily, coloured, smelly and large molecules — exactly the things that make water taste foul or make syrup brown.

So the more surface a piece of carbon has, the more it can hold. Ordinary charcoal keeps the cell structure of the wood, but much of it is clogged with tar left from the burn, and its pores are large. Activation cleans out the tar and eats new, much finer passages into the carbon walls:

  • Steam (physical) activation. At 800–950 °C — bright orange to yellow heat — steam reacts with carbon: carbon + water → carbon monoxide + hydrogen. It eats away the most reactive carbon first, which honeycombs the walls with pores a few millionths of a millimetre across. You deliberately burn off 30–50% of the charcoal's weight.
  • Chemical activation. Raw (uncharred) wood or shell is soaked in a strong dehydrating chemical — zinc chloride or phosphoric acid — and then charred at a lower heat, 450–600 °C. The chemical pulls water out of the wood as it chars and props the structure open; washing it out afterwards leaves the pores behind.

Good activated carbon has an inner surface of 500–1,500 square metres per gram. Ordinary charcoal has perhaps a tenth as much.

What it does not do matters as much. Activated carbon does not remove dissolved salts, nitrates or most metals, does not reliably remove germs (bacteria even grow inside old filters), and does not hold small molecules like alcohol, methanol, carbon monoxide, ammonia or iron. When its surface is full it stops working, and has to be replaced or reheated.

Small boileron its own fire Steamgentle: a cupful ofwater every 10–15 min Charcoal in an iron pipe1–2 cm pieces; the steam passingthrough eats pores into them FlareCO + hydrogen,keep it lit Bright orange, 800–900 °Cfor 1½–3 hours, then cool sealed overnight Clay-luted capno air must get in
Fig. 1 Steam activation. Charcoal in an iron pipe is held at bright orange heat while steam from a water boiler passes through it. The steam eats into the carbon and comes out as carbon monoxide and hydrogen, which are burned off in a small flare at the outlet.

What you need

Item Amount Notes
Dense charcoal 5–10 kg per run Best from coconut shell, nutshells, fruit stones or dense hardwood. Made in a closed retort (Charcoal, Method 3).
Activation retort 1 Iron pipe 8–12 cm across, about 1 m long, ends closed with screwed or clay-luted caps, a small inlet pipe at one end and an outlet at the other (Sheet Metal and Rolling, Metal Casting). Or a large fireclay tube (Firebrick and Refractories).
Furnace 1 A brick or clay firebox that can hold the middle 60 cm of the pipe at bright orange heat for hours — a forge with Bellows, or a charcoal or Coal and Coke fire in a channel of bricks (The Kiln).
Steam supply 1 A small closed iron kettle or pot with a lid and a pipe, on its own fire; or a thin iron tube dripping water into the hot inlet end.
For chemical activation Zinc chloride (zinc dissolved in Hydrochloric Acid, see Zinc and Brass) or phosphoric acid (from bone ash, see Phosphoric Acid and Phosphates); glazed pots
Mortar, sieves, cloth For grinding and sizing

Where to find it

  • Coconut shell makes the best carbon there is: hard, dense, full of very fine pores. On tropical coasts the shells are a waste product.
  • Nutshells and fruit stones — walnut, hazelnut, almond, peach, apricot, olive and date stones — are nearly as good. Save them all year.
  • Dense hardwoods — oak, beech, hornbeam, maple, birch, and in the tropics hard woods such as mangrove — give a good general carbon. Light softwoods give a soft, crumbly one.
  • Bones make bone char (bone black): mostly calcium phosphate with about a tenth carbon, the classic sugar decolouriser (Horn and Bone Working).
  • Never use painted, tarred or treated wood, or plastics from ruins: their poisons stay in the carbon.

Method 1: Steam activation

  1. Make the charcoal in a closed retort, so it is clean and fully charred (Charcoal). Break it into pieces 1–2 cm across (for granules) and sieve out the dust.
  2. Load the pipe loosely with charcoal, leaving a little space at each end. Screw on or lute the caps with clay mixed with sand. The inlet pipe at one end connects to the steam supply; the outlet pipe at the other end points up, away from you.
  3. Heat the pipe in the furnace. Bring the middle to bright orange (800–900 °C) — the colour of a forge fire that is ready to weld. It takes about an hour. Keep the steam off until then; until the charcoal is this hot, steam only wets it.
  4. Start the steam slowly — a gentle plume, about a cupful of water boiled away every 10–15 minutes for a 1 m pipe. Too much steam cools the charcoal and wastes fuel.
  5. Light the outlet gas. The gas coming out — carbon monoxide and hydrogen — burns with a pale blue flame. Light it with a burning stick held at arm's length as soon as it starts, and keep it lit. Never let it pour unburned into the air near people.
  6. Hold it for 1½–3 hours depending on the size of the pieces. Small granules activate faster. Keep the furnace steady at bright orange: at dull red nothing happens; at white heat the charcoal burns away too fast.
  7. Shut down. Stop the steam. Plug the outlet and inlet with clay. Let the pipe cool completely, sealed, overnight. Hot activated carbon meeting air can catch fire.
  8. Check the weight. You should get back 50–70% of what you put in. Much more means it was not hot enough; much less means air leaked in and it burned.

Method 2: Chemical activation

This gives excellent carbon at a lower temperature, from sawdust and shell fragments too small for Method 1 — but you need a strong chemical, and must wash it out thoroughly.

  1. Crush dry shells or hardwood to pieces of 2–5 mm, or use fine dry sawdust.
  2. Soak them in an equal weight of chemical, as a strong solution: for example 1 kg of crushed shell in a solution of 1 kg of zinc chloride in about 1 litre of water, or in about 2 litres of 50% phosphoric acid. Use a glazed pot. Stir and leave 12–24 hours.
  3. Drain and dry the soaked material on a glazed tray in the sun or near a fire.
  4. Char it in a closed pot or retort with a small vent (Charcoal, Method 3), at dull to cherry red (450–600 °C), for 1–2 hours after the smoke from the vent stops. Let it cool sealed.
  5. Wash it in hot water again and again — for zinc chloride, first in water with a little Hydrochloric Acid — until the wash water no longer turns red-cabbage juice pink or red (Acids, Bases and Testing). Keep the first washings: boiled down, they give back much of the chemical.
  6. Dry it thoroughly.

Method 3: Bone char

Boil bones to remove fat and glue (Soap, Glues and Adhesives). Dry them, break them into walnut-sized pieces and heat them in a closed pot, as for charcoal, at a red heat for 3–4 hours. They come out black, not white (white bone ash means air got in). Crush to 1–3 mm grains. Bone char is best for decolourising sugar syrup; it can be washed and re-burned many times.

Grinding and sizing

  • Granules of 0.5–3 mm for water filters, columns and respirators. Crush gently in a mortar and sieve out the dust. Wash the granules in clean water until the water runs clear.
  • Fine powder for medicine, sugar and the laboratory: grind in a stone mortar or a The Watermill-driven mill until it feels like flour. Finer powder works faster.
  • Store in tightly closed jars. Open, it slowly fills its pores with smells and damp from the air and loses strength.

Using it

A drinking-water filter

Water poured in gently Clothspreads the water, catches leaves Fine sand, 5–10 cmtakes out mud and specks Carbon granules, 15–25 cm0.5–3 mm, washed; takes out tastes,smells, colour, chlorine, oils Gravel, 5 cmholds the carbon off the outlet Slowabout 1 litreevery 3–5 min Then boil or chlorinate carbon does not make water safe from germs
Fig. 2 A household filter. Water passes slowly through a cloth, a layer of fine sand and a deep bed of carbon granules resting on gravel. It comes out clear and sweet — but not safe from germs until it is boiled or chlorinated.
  1. Take a clay pot, wooden bucket or barrel with a small outlet hole in the bottom (Pottery, Barrels and Cooperage).
  2. Fill from the bottom: 5 cm of washed gravel, 15–25 cm of washed carbon granules, 5–10 cm of fine washed sand, and a cloth on top to spread the water and catch leaves.
  3. Let it run slowly. Water needs several minutes in contact with the carbon. For a bed 25 cm across, aim for about a litre every 3–5 minutes. Narrow the outlet with a wooden peg if it runs faster.
  4. Then disinfect. Boil the filtered water, or add chlorine (Chlorine and Bleach) after the filter — carbon removes chlorine, so chlorine added before it is wasted.
  5. Renew the carbon every 1–3 months, or sooner when the taste or smell comes back. Reheat used carbon as in Method 1 to reuse it.

Whitening sugar syrup

Dissolve raw sugar in its own weight of hot water. At 70–80 °C (too hot to hold a finger in), stir in 1–2% of fine carbon powder by weight of the sugar (10–20 g per kilo) and keep it hot and stirred for 20–30 minutes. Filter through tightly woven cloth, then through paper if you have it (Paper). Boil down and crystallise as in Sugar. Or run the hot syrup slowly through a tall column of bone-char granules.

Smoothing spirits

Run distilled spirit very slowly through a column of granular hardwood charcoal 30–100 cm deep. It removes some harsh, oily flavours. It does not remove methanol. Wood-spirit poisoning is prevented only by careful distillation (Distillation, Ether, Acetone and Solvents).

A simple respirator

A canister about 8–10 cm across and 10 cm deep, packed with 1–3 mm granules between pads of cotton or wool felt, with a mouthpiece or a close-fitting mask of leather and cloth (Hides and Leather, Felt). It adsorbs fumes of turpentine, ether, tar oils and other solvents for a few hours of work. Soaking the granules in soda solution (Soda Ash and Baking Soda) and drying them helps against acid fumes such as sulfur dioxide.

Be honest about its limits:

  • It gives no protection against carbon monoxide, and none at all in smoke, in a closed tank, a well, a mine or anywhere the air may lack oxygen.
  • When you start to smell the fumes, the carbon is full. Leave and replace it.
  • It is a workshop aid, not a way to enter a dangerous atmosphere.

Poisoning

For many swallowed poisons — most medicines and many poisonous plants, berries and mushrooms — a single dose of fine activated carbon in water, given within about an hour, binds the poison in the gut so less reaches the blood.

Who Dose
Adult 50 g of fine powder (roughly half a cup to a cup, depending on how fine it is), stirred into a glass of water
Child 1 g per kg of body weight (a 20 kg child: 20 g)

It must be drunk; stir and give it quickly, as a grey slurry.

Warning When not to give it. Do not give it to anyone who is drowsy, fitting or cannot swallow safely — if they vomit and breathe it in, it ruins the lungs. It is useless for: alcohol and methanol, lye and acids (corrosives — see Emergencies and Emergency Cards), petrol, paraffin and other oils, iron, lithium and most metal salts, and cyanide. Burnt toast does not work: it is not activated, and old "universal antidotes" based on it were worthless. Activated carbon is a first step, never a reason to skip whatever other care exists.

How to tell it worked

  • The fizz test. Drop a few dry granules into a glass of water. Activated carbon hisses and streams fine bubbles for half a minute or more as water pushes air out of the pores. Plain charcoal gives a few bubbles and stops.
  • The colour test. Make a test liquid: strong tea, or one drop of iodine tincture (Iodine) in 100 ml of water. Shake 2 g (a level teaspoon) of powdered carbon with 100 ml of it for two minutes and filter through paper or a cloth with a pad of cotton. Good activated carbon gives water that is nearly colourless. Plain charcoal leaves it clearly tinted. Keep a jar of your best batch and compare each new batch against it.
  • Feel and look. Good steam-activated charcoal is lighter than it was, dull black, and rings faintly when knocked; it does not leave tarry smears on the fingers.

Note Troubleshooting. Little weight lost and a poor colour test → too cool (below bright orange) or too little steam. Hotter and longer. Most of it burned away to ash → air leaked into the pipe; reseal the caps and joints with clay, or the steam supply ran dry and air was drawn in. Charcoal soggy after the run → steam was started before the pipe was hot. Chemically activated carbon tastes salty or sour → not washed enough. Wash again until the wash water is neutral. Filter water tastes musty after a few weeks → the carbon is full and has grown slime. Replace or reheat it, and always boil or chlorinate after filtering.

Dangers

Danger Carbon monoxide. Steam activation turns carbon into carbon monoxide and hydrogen — a poisonous and flammable gas. Work outdoors, keep the outlet flame lit, stand upwind, and stop at once if anyone gets a headache, dizziness or nausea (Fire, Coal and Coke).

  • Self-heating. Freshly made activated carbon, especially still warm, can heat up and smoulder when it meets air. Cool it sealed, and never store warm carbon in sacks or near wood.
  • Oxygen theft. Wet activated carbon in a closed tank, filter vessel or silo slowly takes oxygen out of the air above it. Never climb into such a vessel without airing it for a long time first.
  • Dust. Fine carbon dust is dirty, irritates the lungs, and a cloud of it can catch fire. Grind it damp or under a cover.
  • Chemicals. Zinc chloride and phosphoric acid burn skin and eyes. Wear gloves and eye protection (Acids, Bases and Testing).
  • Used carbon holds what it caught. Do not reheat carbon from a respirator or a poisoning near people or food.

What this unlocks

Safer-tasting water for villages and towns (Water Treatment for a Town); white sugar and cleaner medicines (Sugar, Making Medicines); clean gases for the laboratory (Hydrogen, Oxygen and Gases); protection from solvent and tar fumes (Ether, Acetone and Solvents, Coal Tar Chemicals); and a real treatment for many poisonings. The same porous carbon later carries metal catalysts in chemical works and makes electrodes for batteries (The Battery).

How it was first done

Charcoal was used against foul smells in medicine in ancient Egypt — a papyrus from about 1550 BC mentions it — and charred wood has been used to keep and sweeten water since antiquity. In 1773 the Swedish chemist Carl Wilhelm Scheele noticed that charcoal soaked up gases, and in 1785 Tobias Lowitz in St Petersburg showed that it decolourised solutions. Refiners began clearing sugar with wood charcoal in the 1790s; around 1811–1812 bone char was found to be far better, and it was used in sugar refineries for more than a century.

In 1831 the French pharmacist Pierre-Fleurus Touéry swallowed ten times the deadly dose of strychnine mixed with charcoal before the French Academy of Medicine — and survived. True activation was patented by Raphael von Ostrejko in 1900–1901, with both steam and chemical methods. In 1915, after the first poison-gas attacks of the First World War, the Russian chemist Nikolay Zelinsky designed the activated-charcoal gas mask; in 1918 American children collected peach stones and coconut shells to make carbon for soldiers' masks.

Source: content/entries/chemistry/activated-carbon.md