Mercury

The liquid metal. Roast blood-red cinnabar in closed clay pots and catch the mercury that boils off. Mercury makes thermometers, barometers and the vacuum pumps behind light bulbs and radio valves — and its invisible vapour is one of the most dangerous poisons in this book.

Difficulty
●●●●●
Time
A day to make retorts; half a day per distillation once the retorts are fired
Steps from zero
4 prerequisites →

You need first

Finding and Identifying OresPottery

This unlocks

The Vacuum PumpThe Barometer

Objects made here

retortcondenserbarometer
The full path from nothing — 4 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Finding and Identifying Ores
  4. Pottery
  5. Mercury

Do them roughly in this order. See it on the tech tree →

Why it matters

Mercury is a metal that is liquid at room temperature. It is silver-white, flows like water but beads up like oil, and is 13.6 times heavier than water — a lump of iron floats on it. Those odd properties make it irreplaceable for a handful of instruments that open the door to modern science:

  • Thermometers. Mercury expands evenly with heat and does not wet glass, so a thread of it in a fine glass tube is the classic The Thermometer.
  • Barometers. Air pressure holds up a column of mercury about 76 cm tall. Water would need a tube over 10 m. The mercury The Barometer measures weather, altitude and the weight of the air itself.
  • Vacuum pumps. Falling drops of mercury in a glass tube can pump air out of a bulb until almost nothing is left. Without that, there are no light bulbs and no vacuum tubes (see The Vacuum Pump).
  • Pressure gauges (manometers), U-tubes of mercury that measure steam and gas pressure — and liquid electrical switches and contacts.
  • Amalgams. Mercury dissolves gold, silver, tin and zinc into soft pastes called amalgams. This was used to catch fine gold, to silver mirrors, and to fill teeth. All of these are now known to be dangerous; safer methods are given below.
  • Vermilion. Cinnabar, mercury's ore, ground fine, is the brilliant red pigment vermilion (see Pigments, Paints and Varnish).

Mercury is also deadly. Its vapour poisons the brain and kidneys, and it never breaks down. Make it only if you need it for instruments, make as little as you need, and keep every drop contained.

How it works

Mercury's ore is cinnabar, mercury sulfide (HgS). Heating it frees the mercury in either of two ways:

  • In air, at a dull red heat (about 600 °C), cinnabar burns: its sulfur joins oxygen as sulfur dioxide gas, and the mercury is released.
  • With lime or iron, in a closed pot, the sulfur goes to the lime or iron instead, and the mercury is released with no choking gas. This is the better way.

Either way, mercury boils at 357 °C — well below the heat of the fire — so it leaves the ore as an invisible vapour. All you have to do is lead that vapour to a cool place, where it condenses to liquid droplets, like steam on a cold lid. This is distillation, the same idea as in Distillation, but with a metal.

The whole art is to catch all the vapour. Any that escapes is lost — and poisons whoever breathes it.

What you need

Item Amount Notes
Cinnabar 1–5 kg per run Hand-picked and crushed to pea size
Quicklime or iron filings/scale 1 part to 3 parts ore by weight Lime from Lime; or crushed iron scale from the forge
Clay pots with tight lids, or clay retorts Several Fired, sound, well made. See Pottery
Clay and sand for sealing A bucket Mixed stiff, for luting (sealing) joints
Charcoal or hardwood For a steady red heat
Water in a basin For cooling and to cover the mercury
Chamois leather or tightly woven cloth For cleaning mercury
Thick glass, glazed stoneware or iron bottles For storage
Sulfur powder A jar For spills. See Sulfur

Where to find it

Mercury deposits are rare and occur in particular kinds of places: young volcanic country, hot-spring areas, and along big faults — where hot water has risen through the rock. The famous mines were at Almadén in Spain, Idrija in Slovenia, Huancavelica in Peru, in California's coast ranges, and in Guizhou in China. Cinnabar often comes with white quartz, chalcedony and opal, and sometimes with stibnite or pyrite.

Identifying cinnabar:

  • Colour: bright scarlet to brownish red, in crusts, grains, earthy masses and sometimes small crystals. Stream pebbles can be dark reddish-brown.
  • Streak: scarlet-red on unglazed pottery — brighter than hematite's brownish-red streak.
  • Weight: very heavy, about 8 times water — heavier than galena.
  • Softness: a fingernail nearly scratches it; a copper coin does.
  • Sometimes tiny droplets of liquid mercury sit in cracks and cavities of the ore.

Look-alikes. Realgar (arsenic sulfide) is orange-red with an orange-yellow streak, much lighter, and smells of garlic when heated — and is dangerously poisonous. Hematite has a brownish-red streak and is much harder. Cuprite (a copper ore) is dark red, harder, and gives a green flame.

Tip The tube test — outdoors only. Put a grain of the suspected cinnabar in the closed end of a small glass tube or a narrow clay tube, and heat it in a flame. A grey mirror-like film forms on the cooler part of the tube; rub it with a splinter and it runs together into tiny silver droplets. That is mercury. Do this in the open air, upwind, and do it only once.

Method 1: Two pots, one buried (downward distillation)

This is the simplest method, used in ancient China and the Mediterranean. Mercury vapour is made to go down into a cool pot buried in the ground.

Upper potcinnabar + one-third itsweight of quicklime Fire all rounddull red, 3–4 hours Vapour sinksinto the cool pot Mercurycollects under the water Mouth downore held in by a plugof dry grass Clay sealluting round the joint Earth heaped upkeeps the joint cool Lower pot, buried2–3 cm of water inside
Fig. 1 Downward distillation. Ore and lime in the upper pot are heated by a fire built around it; mercury vapour sinks into the cool lower pot buried in the earth and condenses under water.
  1. Make two pots of well-tempered clay (see Pottery), fired hard and checked for cracks by tapping (a sound pot rings):
    • an upper pot, 15–20 cm tall, with a mouth 6–8 cm across;
    • a lower pot with a mouth that the upper pot's mouth fits exactly into, rim to rim.
  2. Charge the upper pot. Mix crushed cinnabar with one-third its weight of quicklime (or iron scale). Fill the upper pot loosely to two-thirds. Stuff the mouth with a loose plug of dry grass, moss or a perforated clay disc, so the ore cannot fall out when the pot is turned upside down.
  3. Prepare the lower pot. Bury it in the ground up to its rim, in a shady, damp spot. Put 2–3 cm of water in it.
  4. Join them. Turn the upper pot mouth-down onto the lower pot. Seal the joint all round with a thick collar of luting clay — stiff clay mixed with sand and a little dung. Heap earth round the joint and up the lower part of the upper pot, so the joint and lower pot stay cool.
  5. Fire it. Build a fire of charcoal or hardwood round and over the upper pot. Bring it up slowly over half an hour (sudden heat cracks pots), then keep it at a dull red — the upper pot glowing faintly in shade, about 600–700 °C — for 3–4 hours. Do not stand over or downwind of it.
  6. Cool completely. Let the fire die and leave everything until it is cold — overnight. Opening a warm pot releases vapour.
  7. Collect. Dig out the lower pot carefully, outdoors. The mercury lies at the bottom under the water as a heavy silver pool, often mixed with black soot and grey dust (fine mercury droplets coated with dirt). Pour off the water into a basin and keep it; it contains droplets.

Yields vary greatly. Expect to recover half or more of the mercury in the ore once your pots seal well. Cinnabar is 86% mercury, so 1 kg of good hand-picked ore can give several hundred grams.

Method 2: A retort with a condenser

For more control, use a retort: a closed pot heated in a furnace, with a pipe leading the vapour away to a cooled receiver. This is how gold miners recover mercury, and how mercury is best re-purified.

Lid sealed with claydry the luting before firing Sealed potore + quicklime Charcoal firedull red, 2–4 hours Clay pipe1 m or more, sloping down Cold waterpoured on, all the time Wet cloth wrapvapour condenses inside Pipe end1 cm under the water;lift out before cooling Mercury under waterin a basin on a tray
Fig. 2 A clay retort. Ore and lime are heated in a sealed pot; mercury vapour passes along a clay pipe wrapped in wet cloth and drips into a basin of water.
  1. Make the retort. A fired clay pot of 1–3 litres with a lid that fits into a deep rim. Make a hole in the lid, or near the top of the pot, for a clay pipe 2–3 cm in bore and at least 1 m long. Fire the pot and pipe together, or join them with luting clay.
  2. Charge the pot two-thirds full with crushed cinnabar mixed with one-third its weight of quicklime. Seal the lid with luting clay. Let the clay dry for an hour by the fire.
  3. Set up the pot in a simple furnace — a ring of stones or bricks with charcoal round it — with the pipe sloping down away from it into a basin of water. The end of the pipe should dip about 1 cm under the water. Wrap the pipe in wet cloth and keep pouring cold water over it, so the vapour condenses inside.
  4. Heat slowly to a dull red and hold it there for 2–4 hours. Droplets run down the pipe and collect under the water.
  5. Before the fire dies, lift the end of the pipe out of the water (keeping it over the basin). As the pot cools, the gas inside shrinks and would suck cold water back into the hot retort, which can crack it or blow it apart with steam.
  6. Let everything cool fully before opening.

Cleaning and storing mercury

  1. Wash the crude mercury several times in clean water in a basin, pouring off the dirty water each time.
  2. Squeeze it through chamois leather or tightly woven cloth: twist the cloth into a bag and squeeze. Clean mercury comes through in fine bright streams; dirt and amalgams stay in the cloth.
  3. For instrument-grade mercury, re-distil it in a clean retort, alone.
  4. Test it: pure mercury runs over a clean glass plate in round, bright, freely rolling beads that leave no trail. Dirty mercury drags a grey tail and sticks.
  5. Store it in thick glass bottles, glazed stoneware or iron flasks with tight stoppers, under a layer of water, in a cool place, on a tray that would catch a spill, out of reach of children. Mercury was traditionally shipped in iron flasks holding 34.5 kg. Never store it in copper, brass, tin, lead, zinc, gold or silver — it dissolves them.

Uses, and safer alternatives

  • Thermometers and barometers. These need only a few grams to a kilogram of clean mercury, sealed inside glass. Once sealed, they are safe while unbroken. See The Thermometer and The Barometer.
  • Vacuum pumps. The Sprengel pump drops mercury through a fine tube; it gives vacuums good enough for light bulbs and vacuum tubes. See The Vacuum Pump.
  • Gold recovery by amalgam. Mercury rubbed into crushed ore grabs gold; the amalgam is squeezed, then heated to drive the mercury off. If you ever do it, the amalgam must be heated only in a closed retort with a condenser (Method 2). Burning amalgam in an open pan is how small-scale miners still poison themselves and their children. Careful panning and sluicing (Gold and Silver) is the better route.
  • Mirrors. Old mirrors were made by laying tin foil on glass and flooding it with mercury. Workers suffered terribly. Make silvered mirrors instead (see Mirrors).

How to tell it worked

  • A heavy silver liquid that runs in round beads and flows back together. A cupful is so heavy you can barely lift it with one finger through the handle.
  • It does not wet clean glass, paper or your skin (do not test on skin).
  • A drop on clean copper or gold makes a silvery stain that does not wipe off (an amalgam). Use a scrap.
  • Fill a glass tube 1 m long, closed at one end, with clean mercury, close the open end with a finger, turn it upside down into a dish of mercury and remove the finger: the column falls to about 76 cm at sea level, leaving empty space above. That is the The Barometer — and proof you have mercury.

Note Troubleshooting. No mercury at all → pots not sealed (vapour escaped) or not hot enough. Check the luting; hold the dull red longer. Only grey or black powder → that is fine mercury coated with soot and dust ("stupp"). Squeeze it with a little clean mercury through leather, or rub it with wood ash on a slope so the droplets run together. Retort cracked → heated too fast, wet luting, or water sucked back. Heat slowly; lift the pipe out before cooling. Mercury sticky and dull → it contains dissolved metals. Re-distil it. Strong sulfur smell → not enough lime, or air got in. Use more lime; seal better.

Dangers

Danger Mercury vapour poisons without warning. It has no smell and no colour. Even at room temperature, a spill evaporates and fills a closed room with vapour far above safe levels; heated mercury is many times worse. Breathing a heavy dose of hot vapour can destroy the lungs and kill within days. Lower doses over weeks or months cause tremors (shaking hands, shaky writing), irritability, shyness and sudden temper ("mad as a hatter" — hat makers used mercury), memory loss, sore swollen gums, loose teeth, excess saliva, and kidney failure. Unborn babies and children are harmed most. Damage may not fully recover.

Rules for working with mercury:

  1. All heating outdoors, upwind, with nobody downwind, and with the apparatus sealed. Never heat mercury or amalgam in an open dish, ever.
  2. Never heat it indoors. Never keep open mercury in a living space.
  3. Work over a tray with raised edges, on a floor without cracks. A spilled drop shatters into hundreds of tiny beads that roll into every crack and evaporate for years.
  4. Cover it with water whenever it is stored or standing in a dish.
  5. No food, drink or children anywhere near.
  6. Wash hands after any work; though liquid mercury passes through the gut mostly unabsorbed, it is easily spread around.

If you spill it: Get children and pregnant women out. Open windows and doors; leave the room to air for a while if it is warm. Do not sweep (it scatters it) and do not use a vacuum of any kind. Push the beads together with two pieces of stiff paper or card, and pick them up with a dropper or slide them into a jar of water. Shine a light low across the floor to find the last glints. Then sprinkle sulfur powder over the area: it reacts with fine mercury to form harmless-looking black mercury sulfide, which you sweep up after a day and store sealed. Put everything contaminated in a sealed jar.

Danger Never let mercury into water or soil. In mud and water, bacteria turn it into methylmercury, which builds up in fish and in the people who eat them. In the 1950s, at Minamata in Japan, mercury from a factory poisoned thousands of people through fish; many died and children were born with severe brain damage. Bury nothing; pour nothing away. Keep mercury waste sealed.

  • Cinnabar dust and vermilion are less dangerous than vapour, but do not grind them indoors or eat from painted vessels.
  • Sulfur dioxide from open roasting: another reason to use lime and a closed pot.

What this unlocks

With a few hundred grams of clean mercury you can make a The Thermometer and a The Barometer, measure gas pressure for the The Steam Engine, and build a The Vacuum Pump good enough for light bulbs and vacuum tubes. Mercury cups make good electrical contacts in early experiments with the The Electric Motor and The Telegraph. These are precision tools for careful measurement — mercury's real gift.

How it was first done

Cinnabar was used as a red pigment long before anyone made mercury: it coloured burials and wall paintings in Neolithic Turkey and Spain. The Greek philosopher Theophrastus (about 315 BC) described making "liquid silver" by grinding cinnabar with vinegar in a copper mortar, and Roman writers — Vitruvius, Pliny, Dioscorides — described roasting the ore and catching the vapour; the Romans imported cinnabar from Almadén in Spain, which was mined for about two thousand years. The Chinese historian Sima Qian wrote that the tomb of the first emperor, Qin Shi Huang (died 210 BC), held rivers of mercury; soil above the unopened tomb is indeed rich in mercury.

In 1554 Bartolomé de Medina, in Mexico, perfected the patio process, which used mercury to extract silver from ore and made possible the enormous silver output of Spanish America — at a terrible cost to the miners of Huancavelica. Evangelista Torricelli made the first mercury barometer in 1643, Daniel Fahrenheit the first reliable mercury thermometer in 1714, and Hermann Sprengel the mercury vacuum pump in 1865.