◆ Rebuild

Part 7 · Home and Daily Life

Razors, Nail Clippers and Grooming Tools

How to forge, grind, hone and strop a straight razor, make a guarded safety razor, a strop, a shaving brush and shaving soap, nail files, nail clippers and tweezers, hairpins and hair ties, a hand mirror and an ear scoop — and how to keep shared grooming tools from spreading infection.

Difficulty
●●●●●
Time
An afternoon for tweezers, a nail file or hairpins; two or three days to forge, grind and hone a straight razor
Steps from zero
18 prerequisites →

You need first

SteelAxes, Chisels, Knives and PlanesPersonal Hygiene

This unlocks

—
The full path from nothing — 18 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Lye and Potash
  12. Bellows
  13. Soap
  14. Iron (the Bloomery)
  15. Personal Hygiene
  16. Blacksmithing
  17. Steel
  18. Axes, Chisels, Knives and Planes
  19. Razors, Nail Clippers and Grooming Tools

Do them roughly in this order. See it on the tech tree →

Why it matters

Grooming is not vanity. Beards and long hair harbour lice (Personal Hygiene); long, dirty nails carry the germs of diarrhoea from hand to mouth; a splinter left in a finger can become an abscess. Surgeons and nurses need short nails, and tweezers belong in every The First Aid Kit. A razor is also one of the most demanding things a smith can make: if you can make one that shaves, you can make any edge tool.

This chapter builds on Steel, Axes, Chisels, Knives and Planes and Abrasives and Grinding Stones and covers only what is particular to each tool.

How it works

A shaving edge. Hair is tough, about as strong as copper wire of the same thickness. A razor cuts it cleanly only if the edge is very thin and very smooth. Under a lens every edge is a row of tiny teeth: finer stones make them smaller, and stropping on leather straightens and polishes them. A razor that tugs has bent or coarse teeth.

The spine sets the angle. A straight razor is honed lying flat, with both its thick back (the spine) and its edge touching the stone. So the blade's shape fixes the angle: a blade 16 mm wide with a spine 4–4.5 mm thick gives an edge of about 15° included (both sides together). You need not hold an angle, which is why a beginner can hone a razor well.

A thin, springy blade. The faces of a good razor are ground hollow (concave), so behind the edge the steel is very thin and flexes slightly on the beard, following the skin.

What you need

Item For See
High-carbon steel, about 0.8–1.2 % carbon (crucible steel, an old file) Razors, clipper leaves, tweezers Steel
Forge, anvil, files, oil for quenching Forging and hardening Blacksmithing
Small wet grindstone, 10–20 cm across, on a treadle or crank Hollow grinding Abrasives and Grinding Stones
A fine hone (slate, novaculite, fine schist) and a coarser one Setting and finishing the edge Abrasives and Grinding Stones
Vegetable-tanned leather 3–4 mm; linen or canvas Strop Hides and Leather
Horn, bone or hardwood; brass or copper rod Razor scales, pins Horn and Bone Working
Badger, hog or horse hair; pine resin and beeswax Shaving brush Brooms, Brushes and Combs
Tallow, potash and soda lye Shaving soap Soap, Lye and Potash
Brass or steel wire 1–1.2 mm; rubber Hairpins, hair ties Iron and Brass Wire, Rubber
Glass or bronze mirror disc Hand mirror Mirrors

Where to find it

Hones are the key raw material: very fine-grained, even rocks such as dark roofing slate, grey-blue schist, and the white, waxy quartz rock novaculite (Latin for "razor stone"). Rubbed wet with steel, a razor hone feels smooth and slightly slippery yet slowly makes a grey slurry (Abrasives and Grinding Stones). Rouge for the strop is powdered red hematite, levigated (washed and settled) until it feels like nothing between the fingers.

The straight razor

THE STRAIGHT RAZOR, OPEN SECTION THROUGH THE BLADE LYING ON THE HONE Spine4–4.5 mm thick Edgecutting length 7–8 cm Toe Heel Jimps Shank Pivot pin Scales Wedge blade 16 mm wide Spine Hollow grindfaces groundconcave on asmall wheel Edge A thin, hollow-ground blade bends a little and "sings" on the beard. Spine touches Edge touches Both touch, so the spine sets the angle: 4 mm spine, 16 mm blade ≈ 15° included. never lift it
Fig. 1 The straight razor and its parts. Below, the hollow-ground blade in section, and the blade lying on the hone with spine and edge both touching, which fixes the edge angle.

Forging and hardening

  1. Steel. Use the best high-carbon steel you have. Spark-test it (Steel): it should throw bushy, exploding sparks.
  2. Forge the blank: a blade with 7–8 cm of cutting edge and 16 mm wide (narrower is easier at first), a spine 4–4.5 mm thick, the blade drawn thinner and thinner towards the edge, and a narrow shank and tang about 6–7 cm long behind it. Work at an orange heat and stop hammering at dull red.
  3. Normalise three times: heat to cherry red and let it cool in still air. This refines the grain, which matters more in a razor than in anything else.
  4. File the shape, drill a 3 mm pivot hole in the tang, and file a few shallow notches (jimps) under the shank where thumb and finger grip.
  5. Harden at an even cherry red (about 800 °C; a magnet no longer sticks), quenched edge-first into warm oil. Thin blades crack in water.
  6. Temper to a pale straw colour (about 200–220 °C). Polish a strip bright first so you can see the colour run, and quench in oil the moment it arrives.

Grinding

  1. Hollow grind on a small wet grindstone, 10–20 cm across, running towards you through a water trough. Hold the blade flat against the face of the wheel, spine and edge both touching, and sweep it from heel to toe. The small wheel leaves each face concave. Grind both sides equally until the edge is a fine line about 0.2–0.3 mm thick.
  2. Never let the steel get too hot to hold. If straw, brown or blue colours appear at the edge, the temper is gone there; grind it back and re-harden.
  3. Polish on a wooden wheel dressed with fine emery, then with rouge.

A beginner can make a flat-ground razor instead: file and stone each face flat, from spine to edge, like a wedge. It shaves well but is stiffer and harder to hone.

Scales

  1. Cut two scales of horn, bone or hardwood, each about 15 cm × 2 cm × 3 mm, and a small wedge of the same, about 5 mm thick, for the far end.
  2. Pin the tang between the scales at one end with a brass rod through washers, peened over (Nails, Rivets and Wire Fasteners), just tight enough that the blade stays where you leave it. Pin the wedge between the scales at the other end.
  3. Check that the closed razor's edge sits inside the scales without touching them. Adjust the wedge if not.

Honing

HONING, FROM ABOVE: EDGE FIRST STROPPING: SPINE FIRST 1. push, edge leading 3. back, edge leading 2. rollover thespine Spineflat on the stone Edge No pressure beyond the razor's own weight. Never turn it over the edge. Equal strokes each side. Leather5–6 cm wide,50–60 cm long,smooth side out Spineleads Edgetrails Handlepull it taut Light strokes;roll over thespine at the end;30–60 laps
Fig. 2 Honing (left): the razor lies flat, edge leading, and rolls over its spine at each end of the stone. Stropping (right): the opposite way, spine leading, on taut leather.
  1. Set the bevel on the coarser hone. Wet the stone. Lay the razor flat on it, spine and edge touching. Push it along the stone edge first, with no pressure beyond the blade's own weight, sweeping from heel to toe so the whole edge meets the stone.
  2. At the end of the stroke, roll the razor over on its spine (never on its edge) and push it back, edge first again. That is one lap.
  3. Do 10–20 laps, then test: drag the edge, very gently, across a wet thumbnail. If it catches and grips along its whole length, the bevel is set. Where it skids, keep honing.
  4. Finish on the fine hone: 30–50 laps with a light slurry, then a few laps on plain water.
  5. Strop (below), then shave.

Hone again only when stropping no longer brings the edge back, usually every few months.

How to tell a good razor

  • It shaves forearm hair just above the skin without pressure.
  • The hanging hair test: hold a single hair by one end and touch it to the edge. A shaving edge cuts it without the hair bending away.
  • It shaves the face without pulling, and stays good for a week of daily shaves with stropping alone.
  • The blade is straight along its length (sight down it), the edge straight with no "smile" or "frown", and the spine not ground thinner than the rest.

The razor strop

  1. Cut a strip of vegetable-tanned cowhide or horsehide 3–4 mm thick, 5–6 cm wide and 50–60 cm long, free of scars. The smooth grain side is the stropping face.
  2. Rivet a ring or a hook to one end and a wooden handle to the other. A second strip of tightly woven linen or canvas beside it is used first, to clean and warm the edge.
  3. Rub the leather hard with your palm until it is warm and slick. Use no oil or only a trace; a greasy strop is useless.
  4. A paddle strop is leather glued to a flat board 30 × 5 cm. Rub one side with rouge for a sharper, faster strop.

Stropping: hang the strop on a hook and hold it taut and level. Lay the razor flat, spine leading, and draw it away from the hook with light pressure. At the end, roll it on its spine and draw it back. Do 10–20 laps on linen and 30–60 on leather before every shave. Never strop edge-first; you will cut the strop.

The safety razor

A safety razor holds a short blade behind a guard — a comb or bar — so the edge sticks out only a fraction of a millimetre and is held at a fixed angle to the skin. Nicks are rare, and anyone can shave quickly.

A re-honable guarded razor (the 1880s design) is within any good smith's reach:

  1. Forge and harden a small blade 4–5 cm long and 1.5 cm wide, wedge-shaped, with a spine, and hone it like a straight razor.
  2. Make a brass or steel holder shaped like a small hoe: a back plate with a slot for the blade, and in front a comb guard of fine teeth whose tips lie just below the line of the edge, about 0.5–1 mm back.
  3. Hold the blade in place with a spring clip or a small screw (Screws, Nuts and Bolts), so it can be taken out for honing and stropping in a holder.
  4. Fix a handle 8–10 cm long at right angles.

The disposable-blade razor (1900s) clamps a blade of strip steel only about 0.1 mm thick between a guard plate and a cap that bends it into a stiffening curve. Its blades need rolled strip steel (Sheet Metal and Rolling), hardening between cold plates to keep them flat, and machine honing: a factory job.

Shaving brush and soap

Shaving brush

  1. Hair. Badger hair holds the most water and makes the richest lather; hog bristle is stiffer and good; horse hair is acceptable. Use hair only from animals that were slaughtered healthy, never from animals found dead, and wash and boil it before use (see Dangers).
  2. Knot. Comb a bundle about 2–2.5 cm across, with all the root ends together and the natural tips outward. Tie the root end very tightly with waxed thread.
  3. Set. Turn a handle about 6 cm tall and 3 cm across with a socket 2 cm deep. Dip the root end of the knot in hot pitch (pine resin melted with a little beeswax, as for pitch-set brushes in Brooms, Brushes and Combs) and push it into the socket. Hide glue is useless here; water dissolves it.
  4. About 5 cm of hair (the loft) should stand above the handle.

A good brush sheds only a few hairs in its first week, then none, and springs back after pressing.

Shaving soap

Shaving soap differs from washing soap in being rich in tallow (beef or mutton fat), which makes a dense, slick, long-lasting lather, and in containing some potash soap, which makes it softer and quicker to lather. Make it by the method in Soap, with fat that is about three-quarters tallow and one-quarter other oil, saponified with lye that is roughly half potash and half soda, and a little less lye than the fat could take, so the bar is mild. Pour into a wooden bowl or tin and cure for 4–6 weeks.

To shave: soften the beard with hot water for two minutes; swirl the wet brush on the soap for 20 seconds; work the lather on the face for a minute; stretch the skin and shave with the grain in short strokes, the razor at about 30° to the skin. A second pass across the grain gives a closer shave. Rinse in cold water; touch nicks with a wet block of alum (see Dyes and Mordants) to stop the bleeding.

Nail tools

Nail file

  • Steel file. Forge a strip of high-carbon steel 15 cm × 1.2 cm × 2 mm, tapered to a rounded point (for cleaning under nails). Cut very fine teeth with a sharp chisel as for any file (Files and Saws), finer on one side, and harden it. A good one smooths a nail edge in a few strokes without tearing it.
  • Emery board. Glue fine emery or sharp sand (Abrasives and Grinding Stones) onto both sides of a strip of thin board or stiff card 18 × 2 cm with hide glue: coarser grit on one side, finer on the other. Cheap enough to give everyone their own.
  • A lump of pumice smooths hard skin on heels.

Nail clippers and nippers

LEVER NAIL CLIPPER (SIDE, ENLARGED) TWEEZERS Press Jawscurved edges,hard, meetingexactly Pinthrough both leaves Campushes the leaf Leverswings round to work Leavesspring steel, sprung apart Rivet about 6 cm Bendone strip foldedround a rod Armsspring temper(blue), 9–12 cm Tipsmeet across their full width slantpoint
Fig. 3 A lever nail clipper (left): two spring leaves riveted at the back, closed by a cam on the lever pressing down on a pin. Tweezers (right): one strip of spring steel folded over.

Lever nail clipper.

  1. Cut two leaves of high-carbon steel strip about 6 cm × 1.2 cm × 1.5 mm.
  2. Bend the front of each so that the two ends meet face to face, and file each into a concave curve about a fingernail wide. Bevel each on its outside so the two edges meet flat, like the jaws of end-cutting pliers.
  3. Rivet the leaves together at the back, bent so that the jaws stand 2–3 mm apart at rest.
  4. Drill a hole through both leaves about 8 mm behind the jaws for a pin 3 mm thick, riveted underneath, its top passing up through the top leaf.
  5. Make a lever 5–6 cm long with a raised cam (bump) near its front end, pivoted on a tiny cross-pin through the top of the pin. Pressing the lever makes the cam push the top leaf down and close the jaws.
  6. Harden the whole clipper, then temper by setting the riveted back end on a hot iron block and watching the colours run forward. When the back turns blue (springy) and the jaws straw (hard), quench.

The jaws must meet exactly along their whole curve: hold them shut against the light and no light should show. A good clipper cuts a sheet of paper cleanly at the tips.

Nail nippers are easier: two forged arms crossing at a riveted pivot, with short, curved, hardened jaws like end-cutting pliers (Hammers, Pliers, Wrenches and Screwdrivers) and a small leaf spring between the handles to open them. They cut thick toenails better than clippers. Nail scissors are in Scissors, Shears and Folding Knives.

Tweezers

  1. Cut a strip of high-carbon steel or hard brass 18–24 cm × 6–8 mm × 0.8–1 mm.
  2. Fold it in the middle round a rod about 3 mm thick, so the two arms are 9–12 cm long and spring apart.
  3. File the ends to the tip you want: slanted (best for splinters), or pointed (fine work). File the inner faces of the tips so they meet across their whole width when gently squeezed.
  4. Harden and temper steel to blue; brass needs only hammering to work-harden it.

A good pair picks up a single hair from a flat table at the first try, and the tips do not cross or splay under pressure.

Hair tools

Hairpins. Cut spring-steel or brass wire 1–1.2 mm thick into 13–15 cm lengths and bend each into a U with legs 6–7 cm long. For grip, crimp the legs into waves between two wavy-toothed blocks clamped in a vice. Round the tips: melt a tiny ball on brass ends, or dip steel ends in shellac or wax, so they do not scratch the scalp. A bobby pin is the same from flattened wire, with the legs sprung tightly together. Hair sticks of bone, horn or wood, 15–18 cm long and 6 mm thick, tapered and polished, hold a bun without any metal.

Hair ties. The simplest is a braided wool or linen cord, or a leather thong with a toggle. For an elastic tie, roll rubber sheet round a greased rod, cure it (Rubber, Elastic and Rubber Thread), and slice the tube into rings 3–5 mm wide. Covering the ring with knitted thread (Knitting, Crochet and Netting) stops it pulling hair.

Hand mirror

  1. Carve or turn a frame of hardwood with a handle 10–12 cm long and a round or oval recess 10–15 cm across and 5 mm deep.
  2. Fit a mirror disc: polished bronze or speculum metal, or silvered glass (Mirrors).
  3. Hold glass in with a thin wooden ring glued into the recess over its edge, or with small brass tabs; back it with felt or card so it does not rattle and the silvering is protected.

A good hand mirror gives a straight reflection of a straight edge held in front of it, with no waves, and no black spots in the silvering.

Ear scoop

A slip of bone, horn or brass 8–10 cm long with a tiny spoon 3–4 mm across at one end, every edge rounded and polished. Use it only at the opening of the ear, where you can see. Earwax normally works its way out by itself; poking deeper pushes wax in and can pierce the eardrum. For blocked ears, put 2–3 drops of warm (not hot) olive oil in the ear daily for a week and let the wax come out on its own. Do not put oil in an ear that is painful, discharging, or has ever had a burst eardrum.

Hygiene of shared tools

Razors, clippers, tweezers and ear scoops easily carry blood or skin to the next user. That spreads hepatitis B and C and HIV, as well as barber's itch (ringworm of the beard), impetigo and boils.

  1. Best: everyone has their own razor, nail clippers, toothbrush and towel.
  2. A barber, nurse or anyone sharing tools washes each tool with soap and hot water and a brush, then boils it for 20 minutes (Sterilising Instruments and Dressings) before the next person. Boiling does not harm the temper of a razor. Never heat a blade in a flame; it ruins the temper.
  3. Strops and brushes cannot be boiled: dry them fully between uses and discard a brush used on infected skin.
  4. Dry every steel tool at once and wipe it with a trace of oil; a razor stored wet loses its edge to rust.
  5. Never shave over sores, boils or rashes.

How to tell it worked

  • Razor: shaves a hanging hair; shaves the face cleanly without pulling.
  • Strop: smooth, flat, unscored; the razor feels a light, even "draw" on it.
  • Clippers: jaws meet with no light between them; cut paper at the tips.
  • Tweezers: pick up a single hair; tips meet across their width.
  • Brush: makes a thick lather in under a minute; sheds no hairs after the first week.

Note Troubleshooting. Razor pulls and stings → edge not fully set or rolled; back to the fine hone, then strop. Edge shaves at one end only → uneven bevel; hone with a slight sweep, or more strokes on the dull part. Razor good after honing, dull next day → too much pressure on the strop, or stropped edge-first; strop lighter, spine first. Edge chips → steel overhardened or temper too low; re-temper slightly darker. Nicks every shave → angle too steep, or skin not stretched; lower the spine, stretch the skin. Clipper won't cut → jaws don't meet; file the inside of the jaws flat until they close fully. Brush sheds → knot not tied tight or not set deep enough; reset in fresh pitch.

Dangers

Danger Shared blades spread blood-borne disease. Hepatitis B, hepatitis C and HIV can pass on a razor, clipper or tweezer with no visible blood on it. Never share them without boiling them first.

Danger Anthrax from shaving brushes. Hair from animals that died of anthrax carries its spores, and shaving brushes have caused deadly anthrax infections of the face. Take hair only from animals that were healthy at slaughter, never from carcasses found dead. Wash and boil it before use, but do not rely on boiling: spores survive it for hours (Sterilising Instruments and Dressings). Choosing healthy animals is the real protection.

  • Open razors cut deeply. Always close a razor after use, store it out of children's reach, and never try to catch a falling razor.
  • Grinding throws stone and steel dust; grind wet and shield your eyes.
  • Ears: do not push anything into the ear canal.

What this unlocks

The skills here — grinding fine edges, spring tempering, making parts that meet exactly — lead to surgical instruments (Medical Instruments, Basic Surgery), scissors (Scissors, Shears and Folding Knives) and fine metalwork (Watches and Small Clocks). Soaps and creams for the skin are in Toothpaste, Shampoo, Perfume and Cosmetics.

How it was first done

The first razors were flakes of obsidian and flint. Copper razors appear in Egypt before 3000 BC, and bronze razors and tweezers are common finds across Bronze Age Europe and the Near East. Roman barbers shaved with an iron novacula, and Roman sites yield many little grooming sets of tweezers, nail cleaner and ear scoop on one ring. In 1770 the French barber Jean-Jacques Perret described a razor with a wooden guard. Benjamin Huntsman's crucible steel, made in Sheffield from the 1740s, gave the even, fine-grained steel that made Sheffield razors famous, and hollow grinding became usual in the 1800s. The Kampfe brothers of New York sold a guarded safety razor in 1880, and King Camp Gillette, with the engineer William Nickerson, began selling thin disposable blades in 1904. Lever nail clippers were patented in the United States in the 1870s and 1880s; Stephen Perry patented the rubber band in London in 1845; and the bobby pin spread in the 1920s with the short "bobbed" hair that gave it its name.

Source: content/entries/home/grooming-tools.md