Part 14 · Electronics and Computing
Germanium, Gallium and Compound Semiconductors
Germanium was the metal of the first transistors because it melts low and purifies easily; gallium, which melts in your hand, is the heart of every LED and laser diode. How to win both from zinc smelter dust, coal ash and aluminium-works liquor, zone-refine and grow them into crystals, make germanium diodes, and — in outline — combine gallium with arsenic and nitrogen into light-emitting chips, with honest warnings about arsenic.
- Difficulty
- ●●●●●
- Time
- Months to collect and concentrate enough residue for a first 100 g of germanium; a week per zone-refining run; years and a team for a working LED line
- Steps from zero
- 44 prerequisites →
This unlocks
Light-Emitting DiodesThe full path from nothing — 44 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Sulfur
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Pottery
- The Kiln
- Hides and Leather
- Bricks
- Lime
- Salt
- Mercury
- Lye and Potash
- Fermentation
- The Wheel and Axle
- Firebrick and Refractories
- Glass
- Bellows
- Saltpeter
- Gears
- The Lathe
- Iron (the Bloomery)
- Copper Smelting
- Sulfuric Acid
- Laboratory Glassware
- The Waterwheel
- Pumps
- Blacksmithing
- Zinc and Brass
- Hydrochloric Acid
- Magnets
- The Battery
- The Vacuum Pump
- Copper Wire
- The Light Bulb
- The Generator
- The Vacuum Tube
- The Electric Arc Furnace
- Pure Silicon
- Semiconductors and the Transistor
- Germanium, Gallium and Compound Semiconductors
Do them roughly in this order. See it on the tech tree →
Why it matters
The first transistor, in December 1947, was germanium, not silicon. Germanium melts at 938 °C instead of silicon's 1,414 °C, does not attack a graphite boat, and gives up its impurities easily when melted and refrozen. A small workshop with a tube furnace and hydrogen can purify it to transistor grade. For fifteen years — hearing aids, pocket radios, the first transistor computers — it was the material of solid-state electronics (Semiconductors and the Transistor).
Gallium melts at 29.8 °C, in the palm of your hand. Alone it is a curiosity; combined with arsenic, phosphorus or nitrogen it makes compound semiconductors, in which electrons crossing a junction give off light. Silicon and germanium cannot do this usefully. Every LED and laser diode is a gallium compound (Light-Emitting Diodes).
This chapter gives germanium crystals and germanium diodes (a crystal-radio detector that never needs searching), germanium for infrared lenses, fibre cores and gamma detectors, gallium as a dopant, and the long road to gallium arsenide wafers and LED chips.
How it works
Where they hide
Neither metal forms useful ores of its own. They travel as guests:
- Germanium sits in zinc ore (sphalerite) at 0.001–0.05 % and is concentrated in certain coals. Smelting or burning drives its oxide into flue dust and fly ash, which may hold 0.05–1 %.
- Gallium follows aluminium. Bauxite holds about 0.005 %, but in the Bayer liquor of an alumina works (Aluminium), which is reused again and again, it builds up to 100–250 mg per litre. It also turns up in zinc residues.
So you harvest them from the waste of zinc works, gasworks, boilers and alumina plants. Start saving those residues long before you need them.
Germanium's volatile chloride
Germanium and chlorine make germanium tetrachloride, a heavy colourless liquid boiling at 86 °C. So germanium can be distilled out of a slurry of dust and acid, as silicon chloride is (Pure Silicon). Arsenic's chloride distils too, but passing chlorine through the mixture turns arsenic into a form that stays behind.
Zone refining
When a molten zone freezes slowly, most impurities stay in the liquid (Pure Silicon). Drag narrow molten zones along a bar again and again and the impurities are swept to the far end. In germanium most impurities are hundreds of times more soluble in the liquid, so a few passes do a great deal.
Compound semiconductors and light
In gallium arsenide gallium (three outer electrons) and arsenic (five) alternate, behaving on average like silicon. But an electron meeting a hole in GaAs drops straight into it and emits light (a direct gap); in silicon the energy goes into heat. The colour is set by the chemistry:
| Crystal | Light | Volts across a lit diode |
|---|---|---|
| Gallium arsenide | Infrared, 870–940 nm, invisible | 1.2–1.4 |
| Aluminium gallium arsenide | Deep red, 650–660 nm | 1.8–2.0 |
| Gallium arsenide phosphide | Red to orange | 1.8–2.1 |
| Gallium phosphide | Yellow-green; red with zinc and oxygen | 2.1–2.4 |
| Indium gallium nitride | Blue, violet, green | 3.0–3.4 |
What you need
| Item | Details |
|---|---|
| Residues | Zinc-works dust (Zinc and Brass), coal fly ash and flue dust (Coal and Coke), spent Bayer liquor (Aluminium) — tens to hundreds of kilograms |
| Chemicals | Strong Hydrochloric Acid; chlorine (Chlorine and Bleach); pure dry hydrogen and nitrogen (Hydrogen, Oxygen and Gases, Liquid Air, Nitrogen and the Noble Gases); carbon dioxide (Lime); caustic soda (Lye and Potash) |
| Glass | An all-glass still with a 60 cm column (Distillation, Laboratory Glassware); fused-quartz tubes 3–5 cm across (Scientific Glassblowing and Glass-to-Metal Seals) |
| Furnace | A tube furnace to 1,300 °C, steady within a few degrees (Electric Kilns and Furnaces) |
| Graphite | Boats and crucibles of purified graphite (Lampblack and Carbon Black, The Electric Arc Furnace) |
| Water | Twice-distilled in glass, many litres |
| Instruments | A sensitive meter (Measuring Electricity, Electronic Test Equipment), a The Microscope, a thermocouple (The Thermometer) |
| For gallium arsenide | Pure arsenic (Arsenic), sealed quartz ampoules, a two-zone furnace, a fume hood |
Where to find it
- Sphalerite: resinous yellow-brown to black crystals with galena in limestone veins (Zinc and Brass). Whether yours carries germanium or gallium you learn only by testing the smelter dust.
- Coal: test the ash and flue dust of every seam; lignite and coal from the margins of seams are the best bets.
- Bauxite: red-brown, earthy or pea-textured rock of hot wet lands (Aluminium).
- Arsenopyrite: silver-white, steel-hard, garlic-smelling when struck (Arsenic).
Test for germanium. Warm 10 g of dust with 30 ml of strong hydrochloric acid in a flask with a bent tube, and distil a few millilitres into cold water. Add chlorine water, make it strongly acid with Sulfuric Acid, and bubble hydrogen sulfide through it in a fume hood. A white precipitate that forms only in strong acid is germanium sulfide — how Clemens Winkler recognised germanium in 1886. Gallium shows two violet lines (417 and 403 nm) in the The Spectroscope when the residue is held in a flame on a platinum wire.
Making germanium
- Concentrate. Roast flue dust at dull red (600–700 °C) to burn out carbon. Weak material can be fumed: heated with a little coke in a closed furnace, it gives off a dust five to ten times richer in germanium.
- Distil the chloride. Roast the dust fully first, so no free metal is left in it, and keep chlorine flowing throughout: acid on arsenic-bearing dust with metal present makes deadly arsine (see Dangers). In a glass or stoneware still in a fume hood, stir the dust with 3 litres of strong hydrochloric acid per kilogram, bubbling chlorine through it the whole time. Heat gently. Acid fumes and germanium tetrachloride come over at about 83–90 °C; condense them through an ice-cooled condenser into chilled strong acid. The chloride, 1.9 times as heavy as water, gathers as an oily layer at the bottom; run it off.
- Purify. Shake it with fresh strong acid saturated with chlorine, separate, and redistil slowly through a packed column, keeping only what comes over at 83–86 °C. Repeat until a drop evaporated on clean glass leaves no trace. It fumes in damp air: keep it under a ground stopper.
- Turn it to oxide. Pour it slowly, stirring, into six to seven times its volume of ice-cold twice-distilled water. White germanium dioxide settles. Filter, wash sparingly (it is slightly soluble), dry, and calcine at 500–600 °C.
- Reduce. Spread the oxide 5–10 mm deep in a graphite boat in a quartz tube in the furnace. Flush with nitrogen for 15 minutes, then pass slow, pure, dry hydrogen, burning it at the outlet. Hold 650 °C for 4–6 hours: the oxide turns to grey powder. Raise to 1,000 °C; it melts into a mirror-bright pool. Let it freeze slowly from one end. Cool under hydrogen and flush with nitrogen before opening.
Germanium, like water, expands by about 5 % as it freezes. Never freeze it in a closed crucible.
The zone refiner
William Pfann built this instrument for germanium at Bell Laboratories in 1951–52.
- Tube: fused quartz, 3–4 cm across, about 1.2 m long, with gas taps at each end.
- Boat: purified graphite, 40–50 cm long, with a groove 2 cm wide and 1.5 cm deep, lightly smoked so germanium does not wet it.
- Heaters: three to six narrow ring heaters — nichrome or molybdenum coils on short alumina sleeves, or turns of a radio-frequency coil — each melting a band 2–3 cm long, spaced about 10 cm apart, so one trip of the carriage makes several passes.
- Carriage: the heaters ride on a sled drawn by a screw from a slow motor with heavy gearing (The Electric Motor, Gears), at 3–10 cm an hour.
Run it: flush with nitrogen, switch to slow hydrogen, and set each zone to 2–3 cm with solid on both sides — the molten zone is brighter, with a mirror surface. Make six to ten passes. Then cut off the last fifth of the bar, where the impurities went, and the first few centimetres, where the few that prefer the solid collected. Return cuttings to the chloride stage.
Testing purity
- Hot-probe test (Pure Silicon): a hot copper point and a cold one, through a meter; on n-type germanium the hot point is positive. Mark the type along the bar.
- Resistivity: solder wires to the ends of a small bar of known size and measure its resistance. Resistivity = resistance × cross-section ÷ length. Perfectly pure germanium has about 47 ohm-centimetres at room temperature; above 20 is excellent. Transistors want n-type of 1–5 ohm-cm, made by adding a dopant on purpose.
- Warmth test: pure germanium conducts noticeably better warmed in the fingers; dirty material hardly changes.
Growing a germanium crystal
Gordon Teal and John Little pulled the first germanium crystals at Bell Laboratories in 1950 by the Czochralski method (Pure Silicon).
- Melt 100–500 g of zone-refined germanium in a graphite crucible under hydrogen or nitrogen, heated by a winding or a radio-frequency coil.
- Dope the melt: for n-type of about 1 ohm-cm, about 2 mg of antimony per 100 g; for p-type, gallium or indium. Too little to weigh: make a master alloy of 1 part antimony in 100 of germanium, crush it, and weigh out a fraction.
- Touch a small seed crystal to the melt until its tip begins to melt.
- Turn the seed at 10–30 turns a minute and lift it at 1–2 mm a minute, adjusting the heat so the crystal grows 2–3 cm across.
- After 5–15 cm, lift it clear and cool over an hour.
A good crystal has flat faces and straight ridges along its length. Lumps and patches of different shine mean many grains. Slice it 0.3–0.5 mm thick with a thin blade fed with abrasive slurry or a diamond-edged wheel (Industrial Diamond and Hard Abrasives, Abrasives and Grinding Stones), lap flat on glass, and etch bright (Semiconductors and the Transistor).
The germanium diode
The point-contact germanium diode was the first mass-produced semiconductor device, made by the million from the 1940s.
- Solder a die of n-type germanium (1–5 ohm-cm), 1–2 mm square, to a brass or nickel stud. Etch its top face clean.
- Make a whisker of tungsten or gold wire 0.05–0.1 mm, bent into an S-spring with a sharp tip, on a second stud. Bring it down until it presses lightly.
- Form it: discharge a capacitor of a few microfarads, charged to 30–50 V, through the contact in the forward direction. The point welds and a tiny p-region forms beneath it. Test; re-form if needed.
- Seal it in a small glass tube with a lead through each end (Scientific Glassblowing and Glass-to-Metal Seals).
It conducts forward from about 0.2–0.3 V — half of silicon's 0.6 V, which makes it more sensitive to weak signals — and blocks reverse up to tens of volts. In a crystal set (Radio) it needs no searching and does not drift.
Making gallium
- Concentrate: bubble carbon dioxide slowly through a side stream of spent Bayer liquor. Aluminium hydroxide falls first; gallium comes down mostly in the last third. Return the early precipitate to the alumina works and keep the last.
- Repeat: redissolve in caustic soda and carbonate again, three to five times, to about 1 % gallium.
- Electrolyse: dissolve the concentrate in strong caustic soda and electrolyse at about 4 V between nickel or stainless steel electrodes in an iron tank kept at 40–50 °C, so gallium deposits as a liquid and drips to the bottom (Electrolysis, Power Supplies and Regulators).
- Clean it by stirring under warm dilute hydrochloric acid, then water.
- Purify by slow freezing: cool the liquid very slowly just below its melting point with a seed crystal on top. Pure gallium crystallises first; pour off the last liquid, which holds the impurities. Repeat.
Handle it right. Gallium expands 3 % on freezing and can split a full glass bottle: store it in soft plastic, never full. It wets glass and skin, leaving grey smears. It destroys aluminium, soaking in and making it crumble — keep it far from aluminium structures. It supercools, staying liquid for days until touched by a crystal.
Compound semiconductors, in outline
Gallium arsenide wafers
Gallium arsenide melts at 1,238 °C, where arsenic tries to boil off at almost one atmosphere. So it is made in a sealed, evacuated quartz ampoule in a two-zone furnace (the horizontal Bridgman method):
- Put gallium in a quartz boat at one end of a heavy-walled quartz tube (2–3 mm walls), and the matching weight of pure arsenic, plus a few per cent, at the other.
- Pump to a hard vacuum (The Vacuum Pump) and seal with an oxy-hydrogen flame (Scientific Glassblowing and Glass-to-Metal Seals).
- Heat the gallium end to 1,240–1,260 °C and the arsenic end to 610–620 °C. Arsenic vapour crosses and dissolves in the gallium.
- Move the furnace a few millimetres an hour so the melt freezes from a seed at one end into a single crystal.
- Cool over a day, and open the ampoule in a fume hood.
Add a little tellurium or silicon for n-type, zinc for p-type. Slice wafers 0.3–0.5 mm thick and lap them — wet only: GaAs dust is arsenic.
The LED chip
An LED chip is a cube of compound semiconductor 0.25–0.35 mm on a side with a p–n junction just under its top surface.
- Infrared first. Seal an n-type GaAs wafer in a quartz ampoule with a little zinc arsenide and heat to 800–850 °C for about an hour. Zinc diffuses a few thousandths of a millimetre in, making a p-type skin. The light is invisible, but a silicon or germanium photocell (Photocells and Sensors) sees it plainly — for remote switches, light-beam alarms and short optical links.
- Visible red. Grow a layer of aluminium gallium arsenide (about 35 % aluminium) on GaAs by liquid-phase epitaxy: a graphite slider carries the wafer under wells of molten gallium saturated with arsenic and aluminium at 800–850 °C, cooled a fraction of a degree a minute, so crystal grows onto the wafer (Lasers describes the slider). Zinc in one well gives the p-layer, tellurium in another the n-layer. Gallium phosphide grown the same way at about 1,000 °C gives green.
Finishing:
- Lap the wafer from the back to about 0.2 mm.
- Evaporate contacts in vacuum (Vacuum Coating and Thin Films): gold with 12 % germanium on the n side, gold with a little zinc on the p side. Alloy them in at about 420 °C for a minute. Keep the top contact a small dot so light escapes.
- Scratch along lines with a diamond and break into chips.
- Mount each in a polished reflector cup on a lead frame (Presses, Punches and Dies) with silver-filled glue or soft solder.
- Bond a gold wire 0.025 mm thick from the top contact to the other lead (Integrated Circuits).
- Encapsulate in a clear resin dome (Petrochemicals and Modern Plastics), or, like the first LEDs of the 1960s, in a metal can with a glass window.
An LED always needs a series resistor: resistance = (supply volts − LED volts) ÷ current. A red LED (1.9 V) at 20 milliamps from 9 V needs (9 − 1.9) ÷ 0.020 ≈ 360 ohms. Without it the LED dies in a flash.
Gallium nitride and white light
Blue light needs gallium nitride, grown in thin layers on polished sapphire (Synthetic Gems) at 1,000–1,100 °C from gallium compound vapours and ammonia, with magnesium for the p-layer and thin indium gallium nitride layers where the light is made. A blue chip under a yellow cerium phosphor (Rare Earths, Cerium and Phosphors) gives white — the LED lamp (Light-Emitting Diodes). It took the world's chip industry thirty years: a distant target.
How to tell it worked
- Germanium bar: bright grey, brittle, glassy fracture; passes the hot-probe and resistivity tests.
- Crystal: single, straight ridges; an etched face shows even planes under the microscope.
- Germanium diode: louder than galena in a crystal set; 10–100 times more forward than reverse current at 1 V.
- Gallium: melts in the hand to a mirror-bright liquid with no grey skin after washing.
- LED chip: lights (or, if infrared, drives a photocell) at the voltage in the table; brightness rises smoothly with current.
Note Troubleshooting. Germanium oxide grey or yellow → iron or arsenic carried over; redistil with more chlorine. Metal will not melt into a pool → oxide left; longer under hydrogen at 650 °C. Zone breaks through or wanders → zone too long or heater too hot. Crystal grows as many grains → pulled too fast or the heat unsteady. Diode conducts both ways → whisker too heavy or surface dirty; re-etch, lighten, re-form. Gallium will not freeze → supercooled; touch it with solid gallium. LED conducts but stays dark → junction too deep or crystal full of defects — or it is infrared.
Dangers
Danger Arsenic and arsine. Arsenic vapour, arsenic dust and GaAs dust are cumulative poisons (Arsenic). Worse is arsine, a colourless gas formed when arsenic compounds meet acid together with zinc, iron or other active metals, or when metal arsenides get damp. High concentrations destroy the red blood cells; headache, dark red urine and jaundice may come hours later. Never put arsenic-bearing residues in acid with metals present. Work only in a working fume hood, grind wet, and collect all arsenic waste as insoluble iron arsenate (Arsenic).
Danger Pressurised ampoules and hydrogen. A GaAs ampoule holds arsenic vapour at about one atmosphere at red heat; a flawed seal or wrong charge bursts it and fills the room with arsenic. Guard the furnace with steel and never stand in line with the tube. Hydrogen mixed with air explodes: flush tube furnaces with nitrogen before and after, burn the outlet gas, and never open a hot tube.
- Chlorine, acid fumes and germanium tetrachloride burn eyes and lungs: fume hood or outdoors (Chlorine and Bleach, Hydrochloric Acid).
- Etching acids, above all hydrofluoric acid: see Semiconductors and the Transistor and Fluorspar and Fluorine Compounds.
- Gallium is of low toxicity but must never touch aluminium.
What this unlocks
- Alloy-junction germanium transistors (Semiconductors and the Transistor), and with them hearing aids, portable Radios and the first transistor The Computers.
- Infrared lenses: germanium is clear from about 2 to 14 micrometres, for heat cameras and the carbon dioxide laser.
- Laser diodes (Lasers) for Fibre Optics; LED displays and lamps (Displays, Printers and Data Storage, Flat Screens: LCD and LED Displays).
- Gamma spectroscopy with large pure germanium crystals cooled in liquid nitrogen (Detecting Radiation, Cryogenics and Superconductors); the most efficient Solar Cells, stacked gallium compounds on germanium.
How it was first done
In 1871 Dmitri Mendeleev predicted "eka-aluminium" and "eka-silicon" to fill gaps in his periodic table. In 1875 Paul-Émile Lecoq de Boisbaudran saw two new violet lines in the spectrum of zinc blende from Pierrefitte in the Pyrenees and isolated gallium — eka-aluminium. In 1886 Clemens Winkler in Freiberg found his analysis of the mineral argyrodite about 7 % short and tracked the missing part down to germanium — eka-silicon.
Both stayed curiosities until wartime radar, when germanium and silicon detectors were made at Purdue University and elsewhere. John Bardeen and Walter Brattain made the point-contact transistor on germanium at Bell Laboratories in December 1947; Teal and Little pulled germanium crystals in 1950, and Pfann invented zone refining in 1951–52. Heinrich Welker showed in 1952 that compounds like gallium arsenide are semiconductors. In 1962 groups at General Electric, IBM and MIT Lincoln Laboratory made gallium arsenide lasers, and Nick Holonyak at General Electric the first visible red LED. Isamu Akasaki and Hiroshi Amano made good p-type gallium nitride in 1986–89, and Shuji Nakamura at Nichia bright blue LEDs in 1993; the three shared the 2014 Nobel Prize in Physics.