◆ Rebuild

Part 1 · Staying Alive

Hides and Leather

How to turn the skin of an animal into rawhide, soft smoked buckskin or tough bark-tanned leather — for clothing, straps, containers, shoes and the bellows of the first furnaces.

Difficulty
●●●●●
Time
Rawhide in 2–3 days; brain-tanned buckskin in 2–4 days of work; bark-tanned leather in 1–12 months
Steps from zero
3 prerequisites →

You need first

Hunting and Trapping

This unlocks

Glues and AdhesivesDraft Animals and HarnessCrutches, Prosthetics and RehabilitationGames and Sports EquipmentBookbindingBelts, Chains and Power TransmissionPacking, Gaskets and SealsPumpsBellowsBags, Backpacks, Wallets and LuggageFootwearHats, Gloves, Scarves and StockingsLeatherwork and Harness-MakingSnowshoes, Skis and Sledges
The full path from nothing — 3 steps before this one
  1. Cordage and Rope
  2. Stone Tools
  3. Hunting and Trapping
  4. Hides and Leather

Do them roughly in this order. See it on the tech tree →

Why it matters

A raw animal skin rots within days in warm weather, or dries as hard as wood. Tanning turns it into leather — a material that stays soft, strong and flexible for years and does not rot. With leather you make clothes, shoes, bags, water containers, ropes and straps, tool sheaths, hinges, harness for animals (Keeping Animals, The Plough), and the airtight bags of Bellows that blow air into furnaces to smelt Copper Smelting and Iron (the Bloomery). Leather cups and flaps are the valves of the first Pumpss; leather belts drive machines.

Skins also give rawhide for lashings, drums and containers, and hide glue for woodwork. Every hide from your Hunting and Trapping is worth keeping.

How it works

Skin has three layers:

Hair and epidermiskeep for a fur; remove forleather and buckskin Dermisthe leather itself: a mat ofcollagen fibres Fat and membranealways scraped off Grainthe smooth top of the dermis — kept for bark leather, scraped off for buckskin hair side flesh side
Fig. 1 A hide in cross-section. Only the middle layer, the dermis, becomes leather. Hair and the thin outer skin are removed from one side; fat and membrane from the other.
  • Hair and epidermis — the thin outer skin with the hair roots.
  • Dermis — the thick middle layer, a dense mat of protein fibres called collagen. This is the part that becomes leather. Its top surface, just under the hair, is the smooth grain.
  • Flesh side — fat, meat scraps and a tough, slippery membrane.

Raw collagen fibres are food for bacteria, and when they dry they glue themselves together into a hard sheet. Tanning prevents both:

  • Brain tanning coats the fibres with fat and oils (from brains, egg yolk or soap) while they are worked and stretched until dry, so they cannot stick together. Smoking then fixes the softness and makes it water-resistant.
  • Bark (vegetable) tanning soaks the hide for weeks or months in water steeped with bark. Bark contains tannins — bitter, astringent chemicals (the dryness you taste in strong tea or unripe fruit) — which bond permanently to the collagen, so it no longer rots and no longer glues itself together. This is true leather, firm and durable.

What you need

Item For Notes
Fresh hide Everything Deer, goat, sheep, cattle, pig. Small hides are easier to learn on
A sharp flake knife Skinning Stone Tools
Fleshing beam Scraping A smooth log 15–20 cm thick, leaned against a tree at waist height
Dull scraper Fleshing, dehairing A deer leg bone split to a blunt edge, a blunt stone, or a hardwood blade
Wood ash and water Loosening hair Optional but faster; see Lye and Potash
Brains Brain tanning One animal's brain is roughly enough for its own hide
Rope or a frame Softening A cord stretched between trees, or a pole frame
Punk wood Smoking Rotten, crumbly wood
Tanning bark Bark tanning Oak, hemlock, chestnut, sumac leaves, acacia
Watertight containers Soaking Pits lined with clay, pottery (Pottery), hollow logs
Animal fat Finishing leather Rendered tallow, marrow fat, neat's-foot oil

Where to find it

  • Hides from your hunting and trapping, or from domestic animals. Deer, goat and sheep skins are thin and easy; cattle hides are thick and heavy.
  • Brains — from the animal's own skull. Split the skull with a stone axe or knock out a hole at the back; scoop out the brain. It freezes or keeps a few days cold, or can be dried in thin patties.
  • Tanning bark. Oak bark is the classic: strip it in spring, when it peels easily, from felled trees or branches 5–20 cm thick. Hemlock, spruce, chestnut, willow, birch and mangrove barks also work, as do the leaves of sumac and the pods of acacia. Tannin test: chew a sliver. A strong drying, puckering feeling in your mouth means plenty of tannin. Dry the bark and break it into small chips or pound it to a coarse powder.
  • Punk wood. Rotten, dry, crumbly wood from old stumps and fallen trunks — it smoulders with thick smoke rather than burning with flame. Pine cones and rotten dry dung also work.

Step 1: Skinning

Skin the animal as soon as possible after killing, while it is still warm. See Hunting and Trapping for butchering.

  1. Cut along the belly from the throat to the tail, lifting the skin with two fingers as you cut, so the blade runs under the skin and not into the meat.
  2. Cut the legs: around each leg just above the hoof or paw, then along the inside of each leg to meet the belly cut.
  3. Peel. Pull the skin back and push your fist between skin and body, working it loose. Use the knife only where it clings, with the edge turned towards the meat, never towards the skin. Every knife cut through the hide becomes a hole.
  4. For bags and bellows, case-skin small animals instead: cut only across the back legs and around the vent, and peel the whole skin off forwards like a sock, leaving a tube.

If you can't work on it at once, dry it flat in the shade, flesh side out, stretched over a frame or pegged out. Or rub plenty of Salt into the flesh side, fold it flesh-to-flesh, and keep it cool. Either keeps for months.

Step 2: Fleshing and dehairing

Pin herewith your belly Dull scraperblunt, never sharp short strokes,away and down Hideflesh side out Smooth beamlog 15–20 cm thick, top at waist height SCRAPERS split deer leg boneground to a blunt edge or a bluntstone
Fig. 2 The fleshing beam. The hide is draped over a smooth log leaned against a tree and pinned with your belly. A dull scraper pushed down the beam strips off membrane — or, on the other side, hair and grain.
  1. Soak a dried hide in water for a day or two until fully soft again.
  2. Flesh it. Drape the hide flesh-side out over the beam, pin the top edge against the beam with your belly, and push the dull scraper down the beam, away from you, in short firm strokes. Remove every scrap of fat, meat and membrane. Fat left on the hide rots and stops tanning chemicals getting in.
  3. Loosen the hair for buckskin or leather (skip this if you want a fur):
    • Ash method: mix wood ash in water to the thickness of thin gravy. Soak the hide in it for 2–5 days, stirring daily, until hair pulls out easily with a gentle tug. The alkali (see Lye and Potash) swells the hide and loosens the hair.
    • Water method: soak in plain water in a warm place for a few days until the hair slips. It is slower and smellier, and risks rot if left too long.
    • Later, with Lime, a pit of slaked lime and water does the same job and was the tanner's standard.
  4. Scrape the hair off on the beam, hair side out. For buckskin, scrape hard enough to remove the grain layer too, until the surface looks evenly fuzzy; tanning oils penetrate much better without it.
  5. Rinse thoroughly. After ash or lime, soak in many changes of clean water (or a stream) for a day or two, until the hide no longer feels slippery and swollen. Leftover alkali spoils brain tanning and bark tanning alike.

Method 1: Rawhide

Rawhide is simply a cleaned hide dried under tension. It is stiff, hard and translucent, very strong, and shrinks as it dries.

  1. Flesh and dehair the hide (or leave the hair on).
  2. Lace it into a pole frame, or peg it flat, and stretch it tight.
  3. Dry it in the shade for 1–3 days.

Uses: cut it in a spiral into long strips (babiche) for lashing — soak them, tie them wet, and they shrink rock-hard (Basic Woodworking). Make drum heads, snowshoe webbing, shields, boxes and folded containers (parfleches). Rawhide is not waterproof: wet, it softens and starts to rot, and dogs and rodents love to eat it.

Method 2: Brain tanning (buckskin)

This gives soft, white-to-golden, breathable buckskin, perfect for clothing, bags and bellows. It is hard physical work but needs no special materials.

  1. Prepare a fleshed, dehaired, grain-scraped, rinsed hide. Wring out as much water as you can by twisting it around a pole or a tree.
  2. Make the brain solution. Mash the brain in about a litre of warm water until it is a smooth, milky soup. Warm it until it feels comfortably hot to your hand — never too hot to hold your hand in (above about 50 °C it starts to cook the hide).
  3. Soak and work the hide in the solution for 15–60 minutes, squeezing and stretching it so the solution penetrates every part.
  4. Wring it out hard, then repeat the soak and wring two or three times.
  5. Soften by stretching as it dries. This is the key step. Pull, stretch and work the hide constantly — over a taut rope, over the top of a post, or laced into a frame and pushed with a blunt stick — until it is completely dry. It goes from wet and stretchy to white, fluffy and soft. A deer hide takes 2–6 hours of steady work.
  6. Fix the stiff spots. Any part that dried without being worked will be hard and crinkly. Wet it, brain it again, and work it dry again.

Substitutes for brains: two or three egg yolks per litre of water, or a strong solution of soap (Soap), or fish oil, work in the same way.

Smoking

Hide, sewn into a bagclosed at the top, open below;20–60 min, then turn it inside out Skirtold cloth or hide, guidesall the smoke inside Punk wood on coalsthick smoke, no flame Pit30 cm wide, 30 cm deep Tripod or branchholds the bag over the pit
Fig. 3 Smoking buckskin. The hide is sewn into a bag and hung over a pit of smouldering punk wood. Only smoke — never flame or strong heat — should reach it.

Unsmoked buckskin goes stiff as cardboard if it gets wet and dries again. Smoking coats the fibres with chemicals from the smoke that keep them from re-sticking, colours the leather golden to brown, and helps keep insects off.

  1. Sew or pin the hide into a tube or bag, open at the bottom, with a skirt of cloth or old hide around the bottom edge to guide the smoke.
  2. Dig a small pit about 30 cm across and 30 cm deep. Make a small fire in it and let it burn down to coals.
  3. Smother the coals with punk wood, so it smoulders with thick smoke and no flame.
  4. Hang the bag over the pit with its skirt around the pit's edge, so all the smoke goes into the hide.
  5. Smoke 20–60 minutes, checking often, until the inside is evenly coloured light tan to golden. Turn it inside out and smoke the other side. If you see flame, put it out at once: heat ruins the hide.

Method 3: Bark (vegetable) tanning

This makes firm, tough, long-lasting leather for soles, straps, belts, harness, containers and bellows. It needs little effort but a great deal of time.

  1. Prepare the hide: flesh, dehair with ash or lime, and rinse thoroughly. Leave the grain on.
  2. Make tan liquor. Fill a container or a clay-lined pit loosely with crushed bark, cover with water, and steep for one to two weeks; or simmer gently for several hours. It turns red-brown and tastes strongly astringent. Drain off the liquor and keep it.
  3. Start weak. Put the hide first into liquor diluted with three or four parts of water. If the first liquor is strong, the surface tans too fast, seals itself, and stops the tannin reaching the middle (this is called case-hardening).
  4. Strengthen gradually. Every few days, move the hide to a stronger liquor, stirring and turning it daily, over two to four weeks.
  5. Layer it. Finally lay the hide in a pit between layers of fresh crushed bark, top it with strong liquor, and leave it. A thin goat or deer skin may be done in one to three months; a thick cattle hide takes six months to a year. As a rough guide, plan on several times the hide's weight in bark over the whole process.
  6. Finish. Rinse, and let it dry slowly in the shade. While it is still damp, rub in warm animal fat or oil on both sides and work it in (this is called currying). Flex and work the leather as it dries.

How to tell it worked

  • Bark leather: the cut test. Cut a thin sliver from the edge and look at the cut face. Fully tanned leather is the same brown colour all the way through. A pale or white streak in the middle means it needs more time in the tan.
  • Buckskin is soft, fuzzy, opaque white or golden, and stretches without tearing. Wet a corner and let it dry: if smoked properly it dries soft again.
  • Rawhide is translucent, stiff and tight as a drum.
  • No smell of rot. Good leather smells of smoke, bark or nothing.

Note Troubleshooting. Hair won't slip → leave it longer in the ash or water, or make the ash solution stronger. Patches of hair or skin slipping on a fresh fur → it began to rot before you started; work faster, keep hides cold. Buckskin dried hard in places → those parts weren't worked continuously while drying; re-brain and soften again. Bark leather pale in the middle → case-hardened or too short a time; it needs weeks more in weak liquor. Leather cracks when bent → it is too dry; work in more fat. Smoked hide is stiff and shrunken → it got too hot; keep flames out.

Dangers

Danger Anthrax. Never skin or handle the hide of an animal you found dead from unknown causes, especially grazing animals (cattle, sheep, goats, deer) that died suddenly with dark blood oozing from the nose or mouth. Anthrax spores in hides and wool cause black, painless skin ulcers and can kill. Hide workers historically died of it. Burn or deeply bury such carcasses and don't touch them.

  • Alkali burns. Ash and lime solutions burn skin and can blind. Wear gloves of old leather, and rinse splashes off at once with lots of water — especially eyes, for at least 15 minutes. See Lye and Potash.
  • Rot and infection. Rotting hides breed bacteria. Keep cuts covered, wash hands well, and don't let flies breed in your soaking pits.
  • Brains and disease. In regions where deer suffer from chronic wasting disease, don't use their brains or spinal cords; use egg yolk or soap. Wear gloves when handling brains if you can.
  • Smoke. Smoking is done outdoors; never smoke hides inside a shelter (see Fire).

What leather unlocks

Leather gives clothes and shoes for cold climates, water bags and buckets, and straps and harness that make animal power possible (Keeping Animals, The Plough). A goatskin taken off whole (case-skinned), with a nozzle tied into the neck, is the simplest bellows ever made — still used in parts of Africa today. With a wooden frame (Basic Woodworking) and a leather side, you get the hinged Bellows that power metal smelting (Copper Smelting, Iron (the Bloomery)). Leather valves and seals make Pumpss work. And boiling rawhide scraps for hours makes hide glue, the woodworker's glue for thousands of years (Glues and Adhesives). To cut, sew and shape finished leather into shoes, bags and harness, see Leatherwork and Harness-Making and Footwear.

How it was first done

Stone scrapers worn by scraping hides are found at sites hundreds of thousands of years old, so people have been working skins for a very long time. Neanderthals in France made smooth bone tools for working hides, called lissoirs, about 50,000 years ago. The Iceman who died in the Alps 5,300 years ago wore clothes and shoes of sheep, goat, cattle, deer and bear skin, prepared with fat and smoke. The oldest known leather shoe, a cowhide moccasin about 5,500 years old, was found in Areni-1 cave in Armenia. Vegetable tanning was well established in ancient Egypt, and the Romans ran large tanneries using oak bark. Brain tanning and smoking were the methods of many North American peoples, whose buckskin was prized by European settlers.

Source: content/entries/survival/leather.md