◆ Rebuild

Part 3 · Metals

Welding

Join steel into one piece by melting the edges together — with a hammer at white heat, with the 3,100 °C flame of oxygen and acetylene, or with an electric arc and a coated rod. Plus cutting thick steel with an oxygen jet, and protecting your eyes, lungs and workshop.

Difficulty
●●●●●
Time
An afternoon to learn to run a bead once the equipment works; months of practice to weld well
Steps from zero
26 prerequisites →

You need first

The Electric Arc FurnaceCalcium Carbide and Acetylene

This unlocks

Metal Pipes and Tubes
The full path from nothing — 26 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Bricks
  13. Lime
  14. The Wheel and Axle
  15. Firebrick and Refractories
  16. Bellows
  17. Gears
  18. Iron (the Bloomery)
  19. Copper Smelting
  20. The Waterwheel
  21. Blacksmithing
  22. Magnets
  23. Copper Wire
  24. The Generator
  25. The Electric Arc Furnace
  26. Calcium Carbide and Acetylene
  27. Welding

Do them roughly in this order. See it on the tech tree →

Why it matters

Before welding, metal parts were joined by bolts, rivets, solder, or a blacksmith's forge weld. Rivets need holes that weaken the plate and leak; forge welds are limited to what fits in a fire and under a hammer. Fusion welding — melting the edges of two pieces and a filler metal into one pool that freezes solid — joins steel of any size, anywhere, into a single piece as strong as the parts.

Welding builds boilers and pressure vessels, ships (Steamships), pipes and pipelines (Pipes, Plumbing and Aqueducts), bridges, building frames (Steel Frames and Tall Buildings), vehicles (The Motor Vehicle, The Tractor), farm machinery and tanks. Just as important, it repairs: a cracked casting, a broken axle, a worn shaft built back up. The oxygen torch also cuts steel 25 cm thick as easily as a saw cuts wood.

How it works

To weld, you need two things:

  1. Concentrated heat. Steel melts at about 1,500 °C. To melt a small spot before the heat soaks away into the rest of the metal, the heat source must be much hotter: a coal fire reaches about 1,500 °C at best; the oxy-acetylene flame reaches about 3,100 °C; the electric arc 3,000–6,000 °C.
  2. Protection from air. Molten steel greedily takes up oxygen and nitrogen from the air, which leave it porous and brittle. The weld pool must be shielded — by flux (a substance that melts into a glassy coat over the metal), by the flame's own gases, or by the gas and slag from an electrode's coating.

There are three routes, in order of difficulty:

Method Heat What you need Best for
Forge welding Coal or charcoal forge, white heat Forge, anvil, flux Iron and mild steel bars, chain, tools
Gas welding Oxygen + acetylene flame Carbide, oxygen, torch Thin steel, pipes, cast iron, brazing, cutting
Arc welding Electric arc 60–200 A of electricity, coated rods Steel plate of any thickness; fast

Method 1: Forge welding (recap)

The method is in Blacksmithing: scarf the ends, heat both to a white, sparkling "welding heat" under a flux, and hammer them together quickly. For steel, use borax as the flux instead of sand: it melts at a lower heat (about 750 °C) and dissolves scale better, so steel can be welded before it burns. Sprinkle it on at bright red, then bring the pieces to welding heat. Forge welding needs no special equipment, but only works for pieces you can heat whole and hammer, and only for iron and the plainer steels.

Method 2: Oxy-acetylene welding and cutting

Carbide generatorlumps dropped into water Gasholderbell floats on water;weights set the pressure Water sealstops flashback Oxygen receiver2–4 bar, filled fromelectrolysis; never oiled pressure gauge Torchmixes the gases sludge of slaked lime acetylene hose oxygen hose keep acetylene under 0.1 bar (1 m of water)
Fig. 1 The gas welding set-up. Acetylene comes from a carbide generator and passes through a water seal that stops any flame running back; oxygen comes from a receiver filled from an electrolysis plant. The torch mixes them at the tip.

The gases

  • Acetylene comes from calcium carbide and water (see Calcium Carbide and Acetylene). Use a carbide-to-water generator — small lumps of carbide dropped into a large tank of water, so the gas stays cool — feeding a floating gasholder (a bell upside down in water). The weight of the bell sets the pressure. Keep acetylene below about 1 metre of water pressure (0.1 bar) in your homemade equipment; well above 1 bar it can explode on its own.
  • Oxygen comes from splitting water by Electrolysis (see Hydrogen, Oxygen and Gases), or in larger amounts from liquid air (Liquid Air, Nitrogen and the Noble Gases). Every kilowatt-hour gives very roughly 100 litres of oxygen, plus twice as much hydrogen. Store it in a gasholder, then pump it into a strong, tested iron receiver at 2–4 bar with a pump that is never oiled (see the dangers).
  • Water seal (flashback arrestor). Between the acetylene supply and the torch, the gas bubbles up through 10–15 cm of water in a closed pot. If the flame runs back up the hose, it stops at the water. Never weld without one; check the water level daily.

The torch

An injector torch has two valves, a mixing chamber, and a copper tip with a single hole. The oxygen, at a few bar, rushes through a small nozzle and sucks the low-pressure acetylene in with it, the way a breath across a straw lifts water. Tips come in sizes: a hole about 0.8 mm for 1 mm sheet, 1.2 mm for 3 mm plate, 1.6–2 mm for 6 mm plate. Hoses can be made of rubber (Rubber) reinforced with cloth.

Lighting and adjusting the flame

  1. Open the acetylene a little and light it with a spark striker (not a match held at the tip). It burns with a smoky yellow flame.
  2. Open the oxygen slowly. The flame shrinks and turns blue-white, with three zones.
  3. Adjust to a neutral flame: a small, sharp, rounded, brilliant inner cone and a clear outer flame, about equal volumes of each gas. This is the flame for welding steel.
Neutralsharp rounded inner cone, equal gases: for steel hottest point: 2–3 mm past the cone tip Carburisingwhite feather round the cone: too much acetylene Oxidisingshort pointed cone, harsh hiss: brass and bronze only Oxygen cutting oxygen jet preheat flamesto bright red steel burns,slag blown out narrowcut (kerf)
Fig. 2 The three flames. Neutral: one clean inner cone — for steel. Carburising: a white feather around the cone — for hard-facing and some cast iron. Oxidising: a short, pointed, hissing cone — for brass and bronze only. Right: oxygen cutting.
  • Carburising flame (too much acetylene): a white feathery zone around the inner cone. It adds carbon to steel and makes it brittle.
  • Oxidising flame (too much oxygen): short, pointed, purple-tinged cone, and a harsh hiss. It burns steel and makes foaming, sparking welds. Used only for brass and bronze.

The hottest point is 2–3 mm beyond the tip of the inner cone. Hold it there, never touching the metal.

Welding steel sheet and plate

  1. Prepare the edges. For metal up to 3 mm thick, butt the square edges with a gap of 1–2 mm. For 3–6 mm, grind or file each edge to a bevel so the two form a V of 60–70°, leaving a 1–2 mm flat at the bottom. Clean off rust, paint and grease.
  2. Tack the pieces together with small welds every 5–10 cm, so they cannot pull out of line as they heat.
  3. Choose the rod. Use clean, soft mild steel wire, with a diameter of about half the plate thickness plus 1 mm.
  4. Make the pool. Hold the torch at 60–70° to the work, pointing along the joint in the direction you will travel. Play the flame on the start until both edges melt into one shining, liquid pool about 5 mm across.
  5. Add rod and move. Hold the rod at 30–40° to the work, ahead of the torch. Dip its end into the front of the pool (not into the flame), withdraw, move the flame forward a little, dip again. Work right to left (if right-handed) with a steady rhythm. The pool should stay the same size, and the bead should come out evenly rippled, slightly raised, with the metal melted right through to the back.
  6. Finish by lifting the flame slowly so the last pool does not crack.

Speed and size. On 3 mm steel, expect to weld about 10–15 cm a minute once practised. A medium tip burns about 300–500 litres of each gas an hour.

Other metals with the gas flame

  • Cast iron: preheat the whole piece to a dull red in a fire, weld with cast-iron rod and a borax-based flux, using a slightly carburising flame, and let it cool very slowly buried in ash. Cast iron cracks if any part cools fast.
  • Braze-welding: for cast iron, brass, and joining unlike metals, melt a bronze or brass rod into the joint under borax flux, without melting the parts themselves. See Soldering and Brazing.
  • Aluminium needs a special flux of mixed chlorides and fluorides and great care, because it gives no warning by changing colour before it melts.

Oxygen cutting

Iron and steel burn in pure oxygen. A cutting torch has a ring of small heating flames round a central hole for a jet of pure oxygen.

  1. Heat the edge of the steel with the heating flames until it is bright red to yellow (about 900 °C).
  2. Press the oxygen lever. The jet sets the hot iron burning; the iron oxide formed melts and is blown out of the bottom of the cut in a shower of sparks.
  3. Move steadily along the line. A good cut is narrow and almost as smooth as a sawn edge.

This works only for iron and ordinary steel. Cast iron, stainless steel, copper and aluminium do not cut this way, because their oxides melt at a higher temperature than the metal, or the metal melts before it can burn, or (copper) it carries the heat away too fast.

Method 3: Electric arc welding

Core wiresoft steel, 3–4 mm Coatingchalk, quartz, fluoritein water glass Gas shieldfrom the burning coating Arcas long as the rod is thick Weld poolrod and plate melted together Slagchip off when cold Finished beadfine even ripples Base metal direction of travel
Fig. 3 Arc welding with a coated rod. The arc melts the rod and the base metal into one pool; the burning coating makes a gas shield and a layer of slag that protect the hot weld from the air.

The power

The welding arc needs about 20–30 V while burning, and 50–80 V with no load to strike it easily, at 60–200 A. A useful rule: about 40 A for each millimetre of rod diameter — 3 mm rod, 100–130 A. That is 2–5 kW, much less than an arc furnace.

Sources, from easiest:

  • An AC welding transformer from an alternating supply (see The Transformer), with a primary for your line voltage and a secondary of a few dozen turns of thick wire giving about 70 V. Make the current adjustable with a sliding iron core or a tapped choke, which also stops the current running away (see The Electric Arc Furnace).
  • A DC dynamo of 60–100 V with a resistor in series. Make the resistor from coils of thick iron wire in open air, with taps every few turns so you can choose the current. It wastes power but works with any dynamo.
  • A water rheostat for quick tests: two iron plates in a barrel of salty water. Moving the plates closer gives more current. It boils and gives off hydrogen; keep it in the open and away from sparks.

The electrodes

A bare steel wire will strike an arc, but its welds are porous and brittle, because the molten metal soaks up air. The coating is what makes arc welding work. As it burns, it gives a cloud of gas that shields the arc, a slag that floats on the weld and protects it while it cools, and substances that steady the arc and clean the metal.

To make coated rods:

  1. Core wire. Draw soft, low-carbon steel into wire 3–4 mm thick (see Iron and Brass Wire). Straighten it and cut it into 35–45 cm lengths.
  2. Coating mix. A starting recipe to experiment with, by weight: chalk or limestone powder 50, fine quartz flour or fine white clay 20, powdered fluorite 15, and if you have it, ferromanganese powder 10 (The Electric Arc Furnace). Sieve all through a fine cloth.
  3. Binder. Stir in water glass (sodium silicate, see Water Glass (Sodium Silicate)) until the mix is like thick cream. Make water glass by melting equal weights of clean sand and soda ash (Soda Ash and Baking Soda) into a glass, crushing it, and boiling it for hours in water until it dissolves into a syrup.
  4. Coat. Dip each wire repeatedly, or press the paste on, to give a coating about half the core's thickness all round, leaving 3 cm bare at one end for the holder. Strike the coating off the tip end to leave 1–2 mm of bare wire.
  5. Dry and bake. Air-dry for a day, then bake at 200–300 °C (hot enough to brown paper slowly) for an hour. Store them somewhere warm and dry — damp rods spatter and give porous welds.

Carbon-arc welding is the older alternative: use a carbon rod (see The Electric Arc Furnace) as the electrode, with the carbon negative on DC, and feed a separate filler rod into the arc as in gas welding. It is slower, but needs no coated rods and is good for thin sheet, cast iron and brazing.

Running a bead

  1. Clamp the earth lead to the work or the steel bench, close to the weld.
  2. Set the current for the rod: 3 mm rod, about 100–120 A.
  3. Strike the arc by scratching the rod end on the work like a match, then lift it at once to about the rod's own thickness (3 mm).
  4. Travel. Tilt the rod about 15–20° back from upright, leaning in the direction of travel, and move steadily so the pool is about twice the rod's width. Feed the rod down as it burns.
  5. Listen. A good arc makes a steady crackle like frying bacon. A loud hiss and popping means the arc is too long; the rod sticking means it is too short or the current too low.
  6. Chip the slag off with a pointed hammer and brush the weld before laying the next run. Thick plate needs several runs, each cleaned.

How to tell it worked

  • Look. A good bead is even in width and height, with fine regular ripples, blending smoothly into the plate with no groove (undercut) along its edges. The back of a butt weld should show the metal melted right through.
  • Bend test. Weld two strips of 6 mm steel end to end. Grind the weld flush, then bend it around a 25 mm bar in a vice with the weld on the outside. A good weld bends double without cracking.
  • Break test. Saw a nick into the weld and break it with a hammer. The broken face should be solid, bright grey metal right through, without holes, black slag or unmelted edges.
  • Pressure test for tanks and pipes: fill with water, pump it to one and a half times the working pressure, and look for seeping. Never test with compressed air.

Note Troubleshooting. Weld full of holes → damp or bare rods, rust or paint on the joint, arc too long, or (gas) an oxidising flame. Bake rods; clean the joint; shorten the arc; adjust the flame. Bead sits on top in a round blob and peels off → too cold: current too low, or travel too fast. Raise the current; slow down. Holes burned through thin sheet → too much heat. Smaller tip or rod, lower current, faster travel; weld in short stitches. Rod sticks to the work → current too low or arc too short. Twist it free at once (it gets red-hot), and raise the current. Weld cracks as it cools → high-carbon steel or cast iron cooled too fast. Preheat, and cool slowly in ash. Torch pops and goes out → tip dirty or overheated, or gas pressures too low. Clean the tip with soft copper wire; cool it in water with a little oxygen flowing. Work pulled out of shape → tack more closely; weld in short sections, jumping from end to end.

Dangers

Danger Arc light and eyes. The welding arc gives off ultraviolet light that burns the eye's surface in seconds ("arc eye": agonising grit-under-the-lids pain 6–12 hours later) and infra-red that can damage the retina permanently. Always look through a dark filter glass in a hood or hand shield: very dark green glass for arc welding (welders' shade 10–12), and lighter green or blue for gas welding (shade 4–6). Make it from glass coloured dark green with iron (see Glass). Test a new glass from several metres away on an arc someone else is striking: the arc should look like a sharp, comfortably dim spark, and leave no bright after-image when you look away. If it dazzles at all, or leaves an after-image, use a darker glass or two layers. Never test home-made glass by looking at the sun: the shade 10–11 used for most welding is too light for it, and home-made glass may let through invisible infra-red that burns the retina without pain. Never use sunglasses or smoked glass. Cover all skin: UV gives a sunburn through thin cotton. Screen off your work so others do not catch a flash.

Danger Fumes. Welding coated or dirty metal can poison you. Galvanised (zinc-coated) steel gives metal-fume fever — shaking and fever a few hours later; cadmium-plated parts can kill; old paint may contain lead. Grind coatings off first, weld in moving air with your head out of the smoke, and never weld parts wet with cleaning solvent.

Danger Acetylene and oxygen. Acetylene above about 1 bar can explode without any spark; keep your system at low pressure. Acetylene forms explosive compounds with copper, silver and mercury: never use copper pipe or brass with much copper, or silver solder, to carry it. Oil and grease burn explosively in pure oxygen: never oil an oxygen valve, pump or fitting, and never handle them with greasy hands. Find leaks with soapy water, never a flame. Shut the gases off at the source when you stop.

Danger Fire and closed containers. Sparks and slag fly 10 m and smoulder for hours. Clear the area of anything that burns; keep water and sand at hand; check the workplace 30 minutes after finishing. Never weld or cut a drum, tank or pipe that has held fuel, oil or any unknown liquid: even a trace of vapour explodes. Fill it completely with water first, or do not do it.

  • Electric shock. 80 V from an AC welder can kill through sweat or wet ground. Keep gloves and clothes dry; stand on dry wood; never change rods with a wet glove. In an emergency, see Emergency Cards.
  • Burns. Wear leather gloves and apron, wool or heavy cotton, and boots. Never wear clothes that melt. Pick up welded pieces with tongs.

What this unlocks

Welding makes possible welded boilers, ships and pipelines, Steel Frames and Tall Buildings, light vehicle frames for the The Motor Vehicle, The Tractor and Gliders and Aeroplanes, and the quick repair of every machine in a community. Hard-facing — welding a layer of hard alloy onto plough points, digger teeth and crusher jaws — makes them last many times longer (see Alloy and Stainless Steels). Railway rails can be joined end to end by thermite welding, in which aluminium powder burning with iron oxide makes liquid iron in a crucible above the joint (see Aluminium and Railways). Electric resistance welding, where a heavy current through two pieces pressed together heats their contact point, makes spot welds for sheet-metal work.

How it was first done

Forge welding is as old as ironworking. Humphry Davy demonstrated the electric arc around 1808–1810. In 1881–1887 Nikolay Benardos, working with Stanisław Olszewski, developed carbon-arc welding and patented it as "Elektrogefest"; in 1888 Nikolay Slavyanov in Russia used a metal rod that melted into the weld. The arc's welds were poor until the Swede Oscar Kjellberg invented the coated electrode around 1907 for repairing ships' boilers. Elihu Thomson in the United States invented resistance welding in 1886. Henry Le Chatelier noted the extreme heat of the oxygen–acetylene flame in 1895, and Edmond Fouché and Charles Picard in France built the first practical oxy-acetylene torch around 1903. Hans Goldschmidt patented the thermite process in 1895. In 1920 the British coaster Fullagar became the first ocean-going ship with an all-welded hull, and during the Second World War welding let American shipyards build thousands of cargo ships, some in a matter of days.

Source: content/entries/metals/welding.md