Part 16 · Reference
Materials Data Tables
Lookup tables for the workshop and laboratory: the periodic table with what each element is used for, melting and boiling points, densities, strengths of wood, stone and metals, heat and temper colours, firing temperatures, wire and sheet gauges, screw threads, dilutions of acids, bleach and brines, food storage times and the energy in fuels.
- Difficulty
- ●●●●●
- Time
- Look up as needed
- Steps from zero
- 4 prerequisites →
This unlocks
—The full path from nothing — 4 steps before this one
- Measurement from Scratch
- Writing and Numbers
- The Scientific Method
- Atoms, Elements and Reactions
- Materials Data Tables
Do them roughly in this order. See it on the tech tree →
How to use this chapter
- These tables gather figures from across the book in one place. Each table links to the chapter that explains the work; read that chapter before you act on a number.
- Temperatures are in °C, densities in grams per cubic centimetre (g/cm³ — the same number as tonnes per cubic metre, and as "times as heavy as water"), strengths in megapascals (MPa = N/mm²). Conversions are in Units, Conversions and Mathematical Tables.
- Natural materials vary. Wood, stone, ore and fuel from your district may differ from the table by a quarter or more. Test your own and write down the results (The Scientific Method).
- Melting and boiling points are for pure substances at sea-level pressure.
The periodic table
Elements in the same column behave alike: the soft metals of column 1 fizz in water and make lye; column 17 makes salts with metals; column 18 is the unreactive gases. Each box gives the symbol and the atomic number. The two rows at the bottom fit into column 3 where the arrows are. Atoms, Elements and Reactions explains the table and how Mendeleev built it, with a full drawing.
| 1 | 2 | 3 | 4 | 5 | 6 | 7 | 8 | 9 | 10 | 11 | 12 | 13 | 14 | 15 | 16 | 17 | 18 |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| H 1 |
He 2 |
||||||||||||||||
| Li 3 |
Be 4 |
B 5 |
C 6 |
N 7 |
O 8 |
F 9 |
Ne 10 |
||||||||||
| Na 11 |
Mg 12 |
Al 13 |
Si 14 |
P 15 |
S 16 |
Cl 17 |
Ar 18 |
||||||||||
| K 19 |
Ca 20 |
Sc 21 |
Ti 22 |
V 23 |
Cr 24 |
Mn 25 |
Fe 26 |
Co 27 |
Ni 28 |
Cu 29 |
Zn 30 |
Ga 31 |
Ge 32 |
As 33 |
Se 34 |
Br 35 |
Kr 36 |
| Rb 37 |
Sr 38 |
Y 39 |
Zr 40 |
Nb 41 |
Mo 42 |
Tc 43 |
Ru 44 |
Rh 45 |
Pd 46 |
Ag 47 |
Cd 48 |
In 49 |
Sn 50 |
Sb 51 |
Te 52 |
I 53 |
Xe 54 |
| Cs 55 |
Ba 56 |
57–71 ↓ |
Hf 72 |
Ta 73 |
W 74 |
Re 75 |
Os 76 |
Ir 77 |
Pt 78 |
Au 79 |
Hg 80 |
Tl 81 |
Pb 82 |
Bi 83 |
Po 84 |
At 85 |
Rn 86 |
| Fr 87 |
Ra 88 |
89–103 ↓ |
Rf 104 |
Db 105 |
Sg 106 |
Bh 107 |
Hs 108 |
Mt 109 |
Ds 110 |
Rg 111 |
Cn 112 |
Nh 113 |
Fl 114 |
Mc 115 |
Lv 116 |
Ts 117 |
Og 118 |
| La 57 |
Ce 58 |
Pr 59 |
Nd 60 |
Pm 61 |
Sm 62 |
Eu 63 |
Gd 64 |
Tb 65 |
Dy 66 |
Ho 67 |
Er 68 |
Tm 69 |
Yb 70 |
Lu 71 |
|||
| Ac 89 |
Th 90 |
Pa 91 |
U 92 |
Np 93 |
Pu 94 |
Am 95 |
Cm 96 |
Bk 97 |
Cf 98 |
Es 99 |
Fm 100 |
Md 101 |
No 102 |
Lr 103 |
The elements: properties and uses
Atomic weights are the standard values, rounded; a number in square brackets is the mass of the longest-lived form of an element that has no stable form. Densities are at room temperature; for gases (marked g/L) they are grams per litre at 0 °C and sea-level pressure. Boiling points above about 2,000 °C differ between handbooks by up to 200 °C; they matter only in vacuum work.
| Z | Symbol | Element | Atomic weight | Melts (°C) | Boils (°C) | Density | What it is used for |
|---|---|---|---|---|---|---|---|
| 1 | H | Hydrogen | 1.008 | −259 | −253 | 0.0899 g/L | Lightest gas; burns to water. Hydrogen, Oxygen and Gases, Ammonia, Airships |
| 2 | He | Helium | 4.003 | — (stays liquid) | −269 | 0.179 g/L | Light, unburnable gas for balloons; coldest liquid. Cryogenics and Superconductors |
| 3 | Li | Lithium | 6.94 | 180 | 1,330 | 0.534 | Lightest metal; batteries. Lithium Batteries |
| 4 | Be | Beryllium | 9.012 | 1,287 | 2,469 | 1.85 | Light, stiff metal; copper alloy springs. Dust is deadly to breathe |
| 5 | B | Boron | 10.81 | 2,076 | 3,927 | 2.34 | Borax for flux, glass and glazes. Borax and Boric Acid |
| 6 | C | Carbon | 12.011 | sublimes about 3,640 | — | graphite 2.2, diamond 3.51 | Charcoal, coke, graphite, diamond; the element of steel and of life. Charcoal, Steel, Industrial Diamond and Hard Abrasives |
| 7 | N | Nitrogen | 14.007 | −210 | −196 | 1.25 g/L | Four-fifths of air; fertiliser. Ammonia, Nitric Acid, Chemical Fertilisers |
| 8 | O | Oxygen | 15.999 | −219 | −183 | 1.43 g/L | A fifth of air; needed for burning and breathing. Hydrogen, Oxygen and Gases, Medical Oxygen |
| 9 | F | Fluorine | 18.998 | −220 | −188 | 1.70 g/L | Fluorides; etching glass. Poison; burns. Fluorspar and Fluorine Compounds |
| 10 | Ne | Neon | 20.180 | −249 | −246 | 0.900 g/L | Red glowing signs. Arc Lamps, Neon and Fluorescent Lights |
| 11 | Na | Sodium | 22.99 | 97.8 | 883 | 0.968 | Salt, soda, lye; reacts violently with water. Sodium and Potassium Metal, Salt, Soda Ash and Baking Soda |
| 12 | Mg | Magnesium | 24.31 | 650 | 1,090 | 1.74 | Light metal; burns with blinding white light. Magnesium |
| 13 | Al | Aluminium | 26.98 | 660 | 2,470 | 2.70 | Light metal that does not rust. Aluminium, Alum and Alumina |
| 14 | Si | Silicon | 28.09 | 1,414 | 3,265 | 2.33 | Sand, glass, chips. Glass, Pure Silicon, Semiconductors and the Transistor |
| 15 | P | Phosphorus | 30.97 | 44.2 | 281 | 1.82 (white) | Fertiliser, matches. White form ignites in air and is poison. Phosphorus |
| 16 | S | Sulfur | 32.06 | 115 | 445 | 2.07 | Sulfuric acid, rubber curing. Sulfur, Sulfuric Acid |
| 17 | Cl | Chlorine | 35.45 | −102 | −34.0 | 3.20 g/L | Bleach, disinfecting water, hydrochloric acid. Poison gas. Chlorine and Bleach, Hydrochloric Acid |
| 18 | Ar | Argon | 39.95 | −189 | −186 | 1.78 g/L | Shielding gas for welding; fills bulbs. Liquid Air, Nitrogen and the Noble Gases, Welding |
| 19 | K | Potassium | 39.10 | 63.5 | 759 | 0.862 | Potash, lye, fertiliser. Sodium and Potassium Metal, Lye and Potash, Saltpeter |
| 20 | Ca | Calcium | 40.08 | 842 | 1,484 | 1.55 | Lime, plaster, cement, bone. Lime, Gypsum and Plaster of Paris, Portland Cement |
| 21 | Sc | Scandium | 44.96 | 1,541 | 2,836 | 2.98 | Small amounts strengthen aluminium; metal-halide lamps |
| 22 | Ti | Titanium | 47.87 | 1,668 | 3,287 | 4.51 | Strong, light, rustless metal; white paint (oxide). Titanium |
| 23 | V | Vanadium | 50.94 | 1,910 | 3,407 | 6.11 | Tough tool steels. Alloy and Stainless Steels |
| 24 | Cr | Chromium | 52.00 | 1,907 | 2,671 | 7.19 | Stainless steel, chrome plating, green and yellow pigments. Chromate salts are poison. Chromium and Its Compounds |
| 25 | Mn | Manganese | 54.94 | 1,246 | 2,061 | 7.21 | Steelmaking, dry cells, purple glass. Alloy and Stainless Steels, Dry Cells and Electric Torches |
| 26 | Fe | Iron | 55.85 | 1,538 | 2,861 | 7.87 | Iron and steel; red and yellow ochre. Iron (the Bloomery), Steel, The Blast Furnace and Cast Iron |
| 27 | Co | Cobalt | 58.93 | 1,495 | 2,927 | 8.90 | Blue glass and glaze; magnets; hard alloys. Nickel and Cobalt |
| 28 | Ni | Nickel | 58.69 | 1,455 | 2,730 | 8.91 | Plating, stainless steel, batteries, coins. Nickel and Cobalt |
| 29 | Cu | Copper | 63.55 | 1,085 | 2,562 | 8.96 | Wire, pipes, bronze, brass. Copper Smelting, Copper Wire, Bronze |
| 30 | Zn | Zinc | 65.38 | 420 | 907 | 7.14 | Brass, galvanising, batteries. Zinc and Brass |
| 31 | Ga | Gallium | 69.72 | 29.8 | 2,400 | 5.91 | Melts in the hand; LEDs. Germanium, Gallium and Compound Semiconductors, Light-Emitting Diodes |
| 32 | Ge | Germanium | 72.63 | 938 | 2,833 | 5.32 | Early transistors; infrared lenses. Germanium, Gallium and Compound Semiconductors |
| 33 | As | Arsenic | 74.92 | sublimes 614 | — | 5.73 | Hardens lead shot; semiconductors. Poison. Arsenic |
| 34 | Se | Selenium | 78.97 | 221 | 685 | 4.81 (grey) | Light cells, red glass, rectifiers. Selenium and Tellurium |
| 35 | Br | Bromine | 79.90 | −7.2 | 58.8 | 3.10 | Dark red liquid; photography, disinfectant. Poison, burns. Bromine and Bromides |
| 36 | Kr | Krypton | 83.80 | −157 | −153 | 3.75 g/L | Lamp gas. Arc Lamps, Neon and Fluorescent Lights |
| 37 | Rb | Rubidium | 85.47 | 39.3 | 688 | 1.53 | Atomic clocks. Atomic Clocks (Overview) |
| 38 | Sr | Strontium | 87.62 | 777 | 1,377 | 2.64 | Colours a flame crimson; ferrite magnets. Permanent Magnets |
| 39 | Y | Yttrium | 88.91 | 1,526 | 3,345 | 4.47 | Lasers, phosphors, superconductors. Rare Earths, Cerium and Phosphors |
| 40 | Zr | Zirconium | 91.22 | 1,855 | 4,377 | 6.52 | Zircon refractories, opaque white glaze. Zircon and Zirconium |
| 41 | Nb | Niobium | 92.91 | 2,477 | 4,744 | 8.57 | Steels; superconducting wire. Alloy and Stainless Steels |
| 42 | Mo | Molybdenum | 95.95 | 2,623 | 4,639 | 10.28 | Tool and high-temperature steels; lubricant (sulfide). Molybdenum |
| 43 | Tc | Technetium | [98] | 2,157 | 4,265 | 11.00 | No stable form; medical imaging only. Radioactive |
| 44 | Ru | Ruthenium | 101.07 | 2,334 | 4,150 | 12.45 | Hard platinum alloys. Palladium, Rhodium and Iridium |
| 45 | Rh | Rhodium | 102.91 | 1,964 | 3,695 | 12.41 | Thermocouples, mirrors. Palladium, Rhodium and Iridium |
| 46 | Pd | Palladium | 106.42 | 1,555 | 2,963 | 12.02 | Catalysts; absorbs hydrogen. Palladium, Rhodium and Iridium |
| 47 | Ag | Silver | 107.87 | 962 | 2,162 | 10.49 | Coins, mirrors, photography; best conductor. Gold and Silver, Silver Nitrate and Silver Salts |
| 48 | Cd | Cadmium | 112.41 | 321 | 767 | 8.65 | Plating, yellow pigment, batteries. Poison. Electroplating |
| 49 | In | Indium | 114.82 | 157 | 2,072 | 7.31 | Low-melting solders; LEDs; clear conducting films. Flat Screens: LCD and LED Displays |
| 50 | Sn | Tin | 118.71 | 232 | 2,602 | 7.27 (white tin) | Tinplate, solder, bronze, pewter. Tin and Pewter |
| 51 | Sb | Antimony | 121.76 | 631 | 1,635 | 6.70 | Hardens lead for type and batteries. Poison. Antimony and Bismuth |
| 52 | Te | Tellurium | 127.60 | 450 | 988 | 6.24 | Thermoelectric coolers, solar cells. Thermocouples and Thermoelectricity |
| 53 | I | Iodine | 126.90 | 114 | 184 | 4.93 | Disinfectant; prevents goitre. Iodine |
| 54 | Xe | Xenon | 131.29 | −112 | −108 | 5.89 g/L | Bright arc lamps, flash tubes. Arc Lamps, Neon and Fluorescent Lights |
| 55 | Cs | Caesium | 132.91 | 28.5 | 671 | 1.93 | Atomic clocks; reacts explosively with water. Atomic Clocks (Overview) |
| 56 | Ba | Barium | 137.33 | 727 | 1,845 | 3.51 | Barite drilling mud, X-ray contrast; soluble salts are poison. Optical Glass and Achromatic Lenses |
| 57 | La | Lanthanum | 138.91 | 920 | 3,464 | 6.16 | Optical glass, lighter flints. Rare Earths, Cerium and Phosphors, Optical Glass and Achromatic Lenses |
| 58 | Ce | Cerium | 140.12 | 795 | 3,443 | 6.77 | Glass polishing, lighter flints, gas mantles. Rare Earths, Cerium and Phosphors |
| 59 | Pr | Praseodymium | 140.91 | 935 | 3,130 | 6.77 | Magnets, yellow-green glass. Rare Earths, Cerium and Phosphors |
| 60 | Nd | Neodymium | 144.24 | 1,024 | 3,074 | 7.01 | Strongest magnets, lasers. Permanent Magnets, Lasers |
| 61 | Pm | Promethium | [145] | 1,042 | 3,000 | 7.26 | No stable form. Radioactive |
| 62 | Sm | Samarium | 150.36 | 1,072 | 1,900 | 7.52 | Heat-resistant magnets. Permanent Magnets |
| 63 | Eu | Europium | 151.96 | 826 | 1,529 | 5.26 | Red phosphor for screens. Rare Earths, Cerium and Phosphors |
| 64 | Gd | Gadolinium | 157.25 | 1,312 | 3,000 | 7.90 | Medical imaging, reactor control. Rare Earths, Cerium and Phosphors |
| 65 | Tb | Terbium | 158.93 | 1,356 | 3,123 | 8.23 | Green phosphor. Rare Earths, Cerium and Phosphors |
| 66 | Dy | Dysprosium | 162.50 | 1,407 | 2,567 | 8.54 | Added to magnets for heat. Rare Earths, Cerium and Phosphors |
| 67 | Ho | Holmium | 164.93 | 1,461 | 2,600 | 8.79 | Lasers. Lasers |
| 68 | Er | Erbium | 167.26 | 1,529 | 2,868 | 9.07 | Fibre-optic amplifiers, pink glass. Fibre Optics |
| 69 | Tm | Thulium | 168.93 | 1,545 | 1,950 | 9.32 | Rare; portable X-ray sources |
| 70 | Yb | Ytterbium | 173.05 | 824 | 1,196 | 6.90 | Rare; lasers, atomic clocks |
| 71 | Lu | Lutetium | 174.97 | 1,652 | 3,402 | 9.84 | Rare; catalysts |
| 72 | Hf | Hafnium | 178.49 | 2,233 | 4,603 | 13.31 | Reactor control rods; chips. Making Microchips |
| 73 | Ta | Tantalum | 180.95 | 3,017 | 5,458 | 16.69 | Capacitors, surgical implants. Resistors, Capacitors and Coils |
| 74 | W | Tungsten | 183.84 | 3,422 | 5,930 | 19.25 | Lamp filaments, hard tools. Tungsten and Filament Wire, The Light Bulb |
| 75 | Re | Rhenium | 186.21 | 3,186 | 5,596 | 21.0 | Jet-engine alloys, thermocouples. Jet Engines |
| 76 | Os | Osmium | 190.23 | 3,033 | 5,012 | 22.6 | Hardest pen nibs; oxide is poison. Palladium, Rhodium and Iridium |
| 77 | Ir | Iridium | 192.22 | 2,446 | 4,130 | 22.6 | Spark plugs, crucibles. Palladium, Rhodium and Iridium |
| 78 | Pt | Platinum | 195.08 | 1,768 | 3,825 | 21.4 | Crucibles, wires, catalysts, thermocouples. Platinum and the Platinum Metals |
| 79 | Au | Gold | 196.97 | 1,064 | 2,970 | 19.30 | Coins, jewellery, contacts. Gold and Silver |
| 80 | Hg | Mercury | 200.59 | −38.8 | 357 | 13.53 | Liquid metal; thermometers, barometers, gold extraction. Poison, vapour too. Mercury |
| 81 | Tl | Thallium | 204.38 | 304 | 1,473 | 11.85 | Rat poison of the past. Deadly poison. Photomultipliers and Scintillation Counters |
| 82 | Pb | Lead | 207.2 | 327 | 1,749 | 11.34 | Pipes, roofs, batteries, radiation shields. Poison. Lead, The Rechargeable Battery |
| 83 | Bi | Bismuth | 208.98 | 271 | 1,564 | 9.78 | Low-melting alloys, medicines. Antimony and Bismuth |
| 84 | Po | Polonium | [209] | 254 | 962 | 9.2 | Radioactive, deadly. Leave alone |
| 85 | At | Astatine | [210] | — | — | — | Radioactive. Exists only in traces |
| 86 | Rn | Radon | [222] | −71 | −61.7 | 9.73 g/L | Radioactive gas that collects in mines, cellars and caves. Detecting Radiation |
| 87 | Fr | Francium | [223] | — | — | — | Radioactive. Exists only in traces |
| 88 | Ra | Radium | [226] | — | — | 5.5 | Old luminous paint. Radioactive, deadly. Leave alone |
| 89 | Ac | Actinium | [227] | — | — | about 10 | Radioactive. Leave alone |
| 90 | Th | Thorium | 232.04 | 1,750 | 4,788 | 11.72 | Old gas mantles, reactor fuel. Radioactive. Lanterns, Gas Lamps and Lighters, Nuclear Energy (Overview) |
| 91 | Pa | Protactinium | 231.04 | — | — | 15.4 | Radioactive. Leave alone |
| 92 | U | Uranium | 238.03 | 1,132 | 4,131 | 19.10 | Reactor fuel; old yellow-green glass and orange glazes. Radioactive. Nuclear Energy (Overview) |
Elements 93 to 118 are made artificially in nuclear reactors and accelerators. None is needed for anything in this book.
Danger Radioactive things: leave them alone. Anything marked with the three-bladed radiation symbol, old luminous dials and instruments painted with radium, the sources inside smoke detectors, and medical or industrial sources: do not open, cut, burn or carry them. Mark the place, keep people away, and read Detecting Radiation. Old gas mantles and uranium glass are weakly radioactive; do not crush them or breathe their dust.
Warning Poisons in the table. Beryllium, arsenic, cadmium, mercury, thallium and lead, and their compounds, poison slowly or quickly. Work them only with the precautions in their own chapters, never with food tools, and never heat them indoors.
Melting points and densities of everyday materials
| Material | Melts or changes (°C) | Density (g/cm³) | Notes |
|---|---|---|---|
| Ice | 0 | 0.917 | Floats; water grows about 9 % on freezing |
| Water | boils 100 at sea level | 1.000 | Boiling falls with height: see the table below |
| Sea water | freezes about −2 | 1.025 | About 3.5 % salt |
| Beeswax | 62–64 | 0.96 | A lower or wider range means it is mixed (Waxes: Beeswax, Plant Waxes and Paraffin) |
| Paraffin wax | 48–62 (soft to hard grades) | 0.9 | Waxes: Beeswax, Plant Waxes and Paraffin, Petroleum and Refining |
| Sulfur | 115 | 2.07 | Sulfur |
| Sugar (sucrose) | melts and browns about 186 | 1.59 | Sugar |
| Bismuth–tin alloy (58 : 42) | 138 | 8.6 | Low-melting alloy (Antimony and Bismuth) |
| Pewter | 170–230 | 7.3 | Mostly tin (Tin and Pewter) |
| Tin–lead soft solder | from 183 | 8.5 | Soldering and Brazing |
| Tin | 232 | 7.27 | Tin and Pewter |
| Type metal | poured at 300–350 | about 10 | Printing |
| Lead | 327 | 11.34 | Lead |
| Zinc | 420 (boils 907) | 7.14 | Zinc and Brass |
| Aluminium | 660 | 2.70 | Aluminium |
| Glass, ordinary (soda-lime) | softens about 700; works at 1,000–1,100 | 2.5 | Glass |
| Salt (sodium chloride) | 801 | 2.17 | Salt |
| Brazing spelter (copper 50 : zinc 50) | about 870 | about 8.2 | Zinc and Brass |
| Lead oxide (litharge) | 888 | 9.5 | Lead glazes melt at 900–1,000 (Glazes) |
| Brass (copper 70 : zinc 30) | 915–955 | 8.5 | Zinc and Brass |
| Silver | 962 | 10.49 | Gold and Silver |
| Bronze (copper 90 : tin 10) | fully liquid about 1,000 | 8.8 | Bronze |
| Gold | 1,064 | 19.30 | Gold and Silver |
| Copper | 1,085 | 8.96 | Copper Smelting |
| Cast iron (3–4.5 % carbon) | 1,150–1,200 | 7.2 | The Blast Furnace and Cast Iron |
| Steel | 1,370–1,520 (more carbon, lower) | 7.85 | Steel |
| Iron, pure or wrought | 1,538 | 7.87 | Cannot be melted in a simple furnace (Iron (the Bloomery)) |
| Platinum | 1,768 | 21.45 | Platinum and the Platinum Metals |
| Silica (quartz, sand) | about 1,710 | 2.65 | Fused Quartz and Halogen Lamps |
| Alumina | 2,072 | 3.95 | Alum and Alumina, Firebrick and Refractories |
| Quicklime (calcium oxide) | 2,613 | 3.34 | Limestone burns to quicklime at 900–1,000 °C (Lime) |
| Magnesia (magnesium oxide) | 2,852 | 3.58 | Firebrick and Refractories |
| Tungsten | 3,422 | 19.25 | Highest melting metal (Tungsten and Filament Wire) |
Liquids:
| Liquid | Boils (°C) | Density (g/cm³) | Notes |
|---|---|---|---|
| Acetone | 56 | 0.79 | Burns easily (Ether, Acetone and Solvents) |
| Methanol (wood alcohol) | 65 | 0.79 | Poison: as little as 15–30 mL can kill or blind, and less has blinded people (Distillation) |
| Ethanol (drinking alcohol) | 78 | 0.79 | Distillation, Spirits, Sake and Liqueurs |
| Water | 100 | 1.00 | — |
| Acetic acid, pure (glacial) | 118; freezes at 17 | 1.05 | Vinegar is 4–8 % (Vinegar and Pickling) |
| Turpentine | 150–180 | 0.86 | Tar, Pitch and Glue, Ether, Acetone and Solvents |
| Petrol (gasoline) | 30–200 | 0.72–0.75 | Petroleum and Refining |
| Kerosene (paraffin oil) | 150–300 | 0.78–0.81 | Petroleum and Refining |
| Diesel | 180–360 | 0.82–0.85 | Petroleum and Refining |
| Glycerine | 290 | 1.26 | Soap |
| Sulfuric acid, 98 % | about 340 | 1.84 | Sulfuric Acid |
| Mercury | 357 | 13.53 | Poison vapour (Mercury) |
| Olive and other plant oils | — | 0.91–0.93 | Oils and Pressing |
| Milk | — | 1.03 | Dairy and Cheese |
Where water boils (it boils about 1 °C lower for every 300 m you climb; see Finding and Purifying Water for boiling times at height and Canning and Bottling for longer processing at height):
| Height above sea level | Air pressure | Water boils at |
|---|---|---|
| 0 m | 101 kPa | 100 °C |
| 300 m | 98 kPa | 99 °C |
| 500 m | 95 kPa | 98 °C |
| 1,000 m | 90 kPa | 97 °C |
| 1,500 m | 85 kPa | 95 °C |
| 2,000 m | 79 kPa | 93 °C |
| 2,500 m | 75 kPa | 92 °C |
| 3,000 m | 70 kPa | 90 °C |
| 4,000 m | 62 kPa | 87 °C |
| 5,000 m | 54 kPa | 83 °C |
Densities of wood, stone and bulk materials
Air-dry wood (about 12–15 % water). Wood lighter than 1.0 floats.
| Wood | Density (g/cm³) | Wood | Density (g/cm³) |
|---|---|---|---|
| Balsa | 0.1–0.2 | Elm | about 0.56 |
| Western red cedar | about 0.37 | Sweet chestnut | about 0.56 |
| Spruce | about 0.45 | Larch | about 0.59 |
| Scots pine | 0.50–0.55 | Birch | about 0.65 |
| Douglas fir | about 0.53 | Ash | about 0.70 |
| Teak | about 0.65 | Oak (European) | 0.65–0.75 |
| Yew | about 0.67 | Beech | about 0.72 |
| Hornbeam | about 0.79 | Hickory | about 0.80 |
| Ebony | 1.0–1.2 (sinks) | Lignum vitae | about 1.25 (sinks) |
| Stone, earth or bulk material | Density (g/cm³) | Notes |
|---|---|---|
| Granite | 2.6–2.8 | — |
| Limestone, marble | 2.5–2.75 | Lime, Stone Masonry |
| Sandstone | 2.2–2.5 | — |
| Basalt | 2.9–3.0 | — |
| Quartz, flint | 2.65 | Stone Tools |
| Concrete | 2.3–2.4 | Mortar and Concrete |
| Fired brick | 1.8–2.0 | Bricks |
| Bone | about 1.9 (solid part) | Horn and Bone Working |
| Dry sand, loose | 1.5–1.7 | Grains and air together |
| Earth, loose | 1.2–1.5 | — |
| Wheat, in bulk | 0.75–0.80 | Granaries and Food Storage |
| Rice in the husk (paddy), in bulk | about 0.58 | Granaries and Food Storage |
| Hay, settled | 0.07–0.09 | Hay and Silage |
| Lump charcoal, in bulk | about 0.2–0.25 | Charcoal |
| Cork | 0.12–0.24 | — |
| Air | 0.0012 | — |
Weight of a piece: weight in kg = length × width × thickness in cm × density ÷ 1,000. An oak beam 20 × 20 × 400 cm at 0.7 weighs 20 × 20 × 400 × 0.7 ÷ 1,000 = 112 kg.
Strength of wood, stone and metals
From Strength of Materials, which explains how to design with them. Breaking stress is what a clean test piece takes before it fails; working stress already includes a safety margin for ordinary steady loads. Never design to the breaking figure.
| Material | Breaking stress in tension (MPa) | Crushing stress (MPa) | Stiffness E (MPa) | Safe working stress for design (MPa) |
|---|---|---|---|---|
| Softwood (pine, spruce), along grain | 80–100 (clear wood) | 35–45 | 9,000–12,000 | 6 in bending, 5 in compression |
| Oak, dry, along grain | 90–110 (clear wood) | 45–55 | 10,000–12,000 | 8 in bending, 7 in compression |
| Granite | 7–20 | 100–250 | 50,000 | 4 in compression; none in tension |
| Limestone, sandstone | 2–10 | 20–150 (very variable) | 20,000–50,000 | 1.5–3 in compression |
| Fired brick in lime mortar (as a wall) | almost none | 3–10 | 5,000 | 0.4–1 |
| Concrete, well made | 2–4 | 20–40 | 25,000 | 7 in compression; reinforce for tension (Reinforced Concrete) |
| Cast iron | 150–250 | 600–900 | 100,000–120,000 | 25 in tension, 100 in compression |
| Wrought iron | 300–370 | (yields at 200) | 190,000 | 80 |
| Mild steel | 400–550 | (yields at 250) | 200,000 | 150 |
| Copper, annealed | 210–250 | — | 117,000 | 50 |
Other materials, for comparison (breaking stress in tension; take a safety factor from the table below):
| Material | Breaking stress (MPa) | Stiffness E (MPa) | Notes |
|---|---|---|---|
| Lead | 12–18 | 16,000 | Creeps under steady load; support it |
| Pure aluminium, annealed | 70–100 | 69,000 | Aluminium |
| Aluminium alloy | 250–300 | 70,000 | Composites: Fibreglass, Carbon Fibre and Honeycomb |
| Bronze, cast (10 % tin) | 250–300 | about 110,000 | Bronze |
| Brass (70 : 30), annealed | 300–350 | about 105,000 | Zinc and Brass |
| Glass | 30–70 in practice (scratches weaken it) | 70,000 | Fails without warning |
| Fibreglass, woven, 50 % glass | 200–250 | 15,000–20,000 | Composites: Fibreglass, Carbon Fibre and Honeycomb |
| Situation | Safety factor on breaking strength |
|---|---|
| Steel or wrought iron, steady loads you know well | 3–4 |
| Timber, steady loads | 4–6 (already in the working stresses above) |
| Brittle materials — cast iron, stone, brick, glass | 6–10 |
| Moving machinery, shock and vibration | Double the above |
| Ropes and chains lifting goods | 5–6 |
| Anything that carries or lifts people | 10 or more |
| Boilers and pressure vessels | 5–6, plus a water-pressure test before use (Boilers and Pressure Vessels) |
Ropes, wire and chain — rules of thumb:
| Item | Rule | Chapter |
|---|---|---|
| New three-strand hemp rope, good quality | Safe working load in kg ≈ (diameter in mm)²: 12 mm ≈ 150 kg, 20 mm ≈ 400 kg | Cranes and Lifting |
| Steel wire rope | Breaking load in tonnes ≈ 0.055 × (diameter in mm)²; work at a tenth of that for people | Wire Rope and Cable |
| Wrought-iron chain | Safe working load ≈ 5 kg per mm² of rod, counting both sides of a link: 8 mm rod ≈ 500 kg | Nails, Rivets and Wire Fasteners |
| Wire 2 mm thick, breaking load | Soft iron 95 kg; hard-drawn iron 150–180 kg; hard brass 150–190 kg; spring steel 450–650 kg | Iron and Brass Wire |
Knots weaken a rope, often by a third to a half, and wet, old or sun-rotted rope is far weaker (Knots, Lashings and Rigging).
Hardness of minerals (Mohs scale)
From Rocks and Minerals. Each mineral scratches the ones above it.
| Mohs | Reference mineral | Field test | Examples |
|---|---|---|---|
| 1 | Talc | Greasy; fingernail scratches it very easily | Soapstone, graphite (1–2) |
| 2 | Gypsum | Fingernail scratches it (fingernail ≈ 2.5) | Rock salt (2.5), clay minerals, mica (2.5–3) |
| 3 | Calcite | Copper scratches it (copper ≈ 3); fingernail does not | Limestone, marble, galena (2.5) |
| 4 | Fluorite | Iron nail scratches it easily (nail ≈ 4.5) | Malachite, dolomite (3.5–4) |
| 5 | Apatite | Steel knife scratches it with effort (knife ≈ 5.5) | Hematite and magnetite (5.5–6.5) |
| 6 | Feldspar | Scratches glass; a file scratches it (file ≈ 6.5) | Feldspar in granite, pyrite (6–6.5) |
| 7 | Quartz | Scratches glass and steel easily | Flint, chert, quartzite |
| 8–10 | Topaz, corundum, diamond | Scratch quartz | Emery (corundum) for Abrasives and Grinding Stones |
Heat colours of iron and steel
Judge in shade, always in the same light. From Blacksmithing.
| Colour (seen in shade) | Temperature | What it means |
|---|---|---|
| No glow, but sizzles water | 100–450 °C | Black heat. Looks cold, burns to the bone |
| Faint red, visible only in the dark | 500–550 °C | Too cold to forge |
| Dull "blood" red | 600–700 °C | Stop forging iron. Light finishing blows only |
| Cherry red | 750–800 °C | Hardening heat for steel (Steel) |
| Bright cherry to orange | 850–950 °C | Light forging; bending |
| Orange to yellow | 1,000–1,150 °C | Main forging heat |
| Light yellow to white, sparkling | 1,250–1,350 °C | Welding heat. A few bright star-sparks |
| Fizzing white with many sparks | above 1,350 °C | Burning. The iron is being destroyed |
Temper colours on clean, bright steel, from Steel:
| Colour | Temperature | Use |
|---|---|---|
| Pale straw | about 220 °C | Razors, scrapers, files, engraving tools — hardest, brittle |
| Straw | about 230–240 °C | Knives, wood chisels, drills, plane blades |
| Brown | about 250–260 °C | Punches, scissors, axes for light use |
| Purple | about 270–280 °C | Axes, cold chisels, tools that are struck hard |
| Dark blue | about 290–300 °C | Springs, saws, screwdrivers — tough and springy |
| Pale blue to grey | over 310 °C | Too soft for most tools. Re-harden and start again |
Annealing heats (to soften metal for working, from Iron and Brass Wire and Sheet Metal and Rolling): copper and brass dull red, 500–650 °C, may be quenched; soft iron cherry red, 700–800 °C, cool slowly; high-carbon steel just below cherry red, 680–720 °C, held an hour, cool very slowly.
Firing and process temperatures
Kiln colours, seen through a spy hole into the chamber, from The Kiln. They read slightly differently from the forge table above because the whole chamber glows.
| Colour inside the kiln | Temperature | What it means |
|---|---|---|
| Faint grey-red, only in total darkness | 450–550 °C | Clay is just turning to ceramic |
| Dark, dull red | 550–650 °C | Bonfire level; weak earthenware |
| Dull cherry red | 650–750 °C | Good low-fired pottery |
| Cherry red | 750–850 °C | Strong earthenware |
| Bright cherry to red-orange | 850–950 °C | Lime begins to burn; bricks firing |
| Orange | 950–1,050 °C | Good earthenware, bricks, lime |
| Yellow-orange | 1,050–1,150 °C | Glass melts; copper melts (1,085 °C) |
| Yellow | 1,150–1,250 °C | Stoneware begins; hard for a wood kiln |
| Pale yellow to white | 1,250 °C and above | Needs a very good kiln or bellows |
| Process | Temperature | Chapter |
|---|---|---|
| Gypsum into plaster of Paris | 120–180 °C; ruined ("dead-burnt") above 400–500 °C | Gypsum and Plaster of Paris |
| Charcoal making: wood gives off tar and gas | 280–400 °C; finished at 400–500 °C | Charcoal |
| Quartz in clay changes size suddenly — heat and cool gently here | 573 °C | Pottery, The Kiln |
| Open-fire (pit) pottery | 600–850 °C | Pottery |
| Mould burnout for lost-wax casting | dull red, 600–700 °C | Bronze, Metal Casting |
| Fired bricks | 900–1,000 °C | Bricks |
| Burning lime | 900–1,000 °C held for 4–6 hours or more | Lime |
| Natural cement | 900–1,100 °C for 8–24 hours | Portland Cement |
| Red earthenware | 950–1,100 °C | Glazes, The Kiln |
| Lead glazes melt | 900–1,000 °C | Glazes |
| Glass melting in a crucible | 1,100–1,200 °C | Glass |
| Stoneware and porcelain | 1,250–1,300 °C | Stoneware and Porcelain |
| Ash glazes | 1,220–1,280 °C | Glazes |
| Portland cement clinker | about 1,450 °C | Portland Cement |
For measuring heat without a thermometer by melting cones, see Pyrometric Cones and Kiln Temperature.
Thermal and electrical properties
| Material | Specific heat (J per g per °C) | Expansion (mm per metre for each 100 °C) | Resistivity (Ω·mm²/m at 20 °C) |
|---|---|---|---|
| Water | 4.18 | — | — |
| Wood | about 1.7 | 0.3–0.5 along the grain | insulator when dry |
| Stone, brick, clay | 0.8–0.9 | 0.5–1.0 | — |
| Glass, ordinary | about 0.84 | 0.9 | insulator |
| Borosilicate glass | about 0.83 | 0.33 | insulator |
| Fused quartz | about 0.74 | 0.055 | insulator |
| Concrete | about 0.9 | 1.0–1.2 | — |
| Iron and steel | 0.45 | 1.2 | iron 0.10; mild steel about 0.14 |
| Copper | 0.39 | 1.7 | 0.0172 |
| Brass | 0.38 | 1.9 | 0.06–0.07 |
| Aluminium | 0.90 | 2.3 | 0.0282 |
| Silver | 0.24 | 1.9 | 0.0159 |
| Lead | 0.13 | 2.9 | 0.21 |
| Platinum | 0.13 | 0.9 | 0.106 |
| Tungsten | 0.13 | 0.45 | 0.053 |
| Nichrome (nickel 80 : chromium 20) | about 0.45 | 1.4 | 1.10 |
| Mercury | 0.14 | — | 0.96 |
Two uses of these columns: a rod 1 m long heated by 100 °C grows by the expansion figure in millimetres, so a 10 m iron rail grows about 5 mm between a frosty night and a hot day (Forces, Energy and Heat); and platinum and ordinary glass expand almost equally, which is why platinum wire can be sealed through glass (The Light Bulb). Resistance of a wire = resistivity × length in metres ÷ cross-section in mm² (Copper Wire, Wiring and Electrical Safety).
Wire gauges
Old books and salvaged wire give sizes as gauge numbers. A bigger number means a thinner wire. Always measure the bare metal with calipers or a micrometer (Rules, Squares, Callipers and Gauges) when it matters.
American Wire Gauge (AWG, also called Brown & Sharpe)
Used in North America for copper and aluminium wire. Every 3 gauges roughly halves the cross-section; every 6 gauges roughly halves the diameter. Resistance and weight are for annealed copper at 20 °C, per kilometre of wire.
| AWG | Diameter (mm) | Cross-section (mm²) | Copper: ohms per km at 20 °C | Copper: kg per km |
|---|---|---|---|---|
| 0000 (4/0) | 11.68 | 107.2 | 0.161 | 953 |
| 000 (3/0) | 10.40 | 85.0 | 0.203 | 756 |
| 00 (2/0) | 9.27 | 67.4 | 0.256 | 599 |
| 0 | 8.25 | 53.5 | 0.322 | 475 |
| 1 | 7.35 | 42.4 | 0.407 | 377 |
| 2 | 6.54 | 33.6 | 0.513 | 299 |
| 3 | 5.83 | 26.7 | 0.646 | 237 |
| 4 | 5.19 | 21.2 | 0.815 | 188 |
| 5 | 4.62 | 16.8 | 1.03 | 149 |
| 6 | 4.12 | 13.3 | 1.30 | 118 |
| 7 | 3.66 | 10.5 | 1.63 | 93.8 |
| 8 | 3.26 | 8.37 | 2.06 | 74.4 |
| 9 | 2.91 | 6.63 | 2.60 | 59.0 |
| 10 | 2.59 | 5.26 | 3.28 | 46.8 |
| 11 | 2.30 | 4.17 | 4.13 | 37.1 |
| 12 | 2.05 | 3.31 | 5.21 | 29.4 |
| 13 | 1.83 | 2.62 | 6.57 | 23.3 |
| 14 | 1.63 | 2.08 | 8.29 | 18.5 |
| 15 | 1.45 | 1.65 | 10.45 | 14.7 |
| 16 | 1.29 | 1.31 | 13.17 | 11.6 |
| 17 | 1.15 | 1.04 | 16.61 | 9.23 |
| 18 | 1.02 | 0.823 | 20.95 | 7.32 |
| 19 | 0.912 | 0.653 | 26.41 | 5.80 |
| 20 | 0.812 | 0.518 | 33.31 | 4.60 |
| 21 | 0.723 | 0.410 | 42.00 | 3.65 |
| 22 | 0.644 | 0.326 | 52.96 | 2.89 |
| 23 | 0.573 | 0.258 | 66.78 | 2.30 |
| 24 | 0.511 | 0.205 | 84.21 | 1.82 |
| 25 | 0.455 | 0.162 | 106 | 1.44 |
| 26 | 0.405 | 0.129 | 134 | 1.14 |
| 27 | 0.361 | 0.102 | 169 | 0.908 |
| 28 | 0.321 | 0.0810 | 213 | 0.720 |
| 29 | 0.286 | 0.0642 | 268 | 0.571 |
| 30 | 0.255 | 0.0509 | 339 | 0.453 |
| 32 | 0.202 | 0.0320 | 538 | 0.285 |
| 34 | 0.160 | 0.0201 | 856 | 0.179 |
| 36 | 0.127 | 0.0127 | 1,361 | 0.113 |
| 38 | 0.101 | 0.0080 | 2,164 | 0.071 |
| 40 | 0.080 | 0.0050 | 3,441 | 0.045 |
British Standard Wire Gauge (SWG, Imperial Standard Wire Gauge)
Used in Britain and its former empire for iron, steel and copper wire, and for sheet metal, from 1884 until metric sizes replaced it.
| SWG | mm | SWG | mm | SWG | mm |
|---|---|---|---|---|---|
| 7/0 | 12.70 | 10 | 3.25 | 26 | 0.457 |
| 6/0 | 11.79 | 11 | 2.95 | 27 | 0.417 |
| 5/0 | 10.97 | 12 | 2.64 | 28 | 0.376 |
| 4/0 | 10.16 | 13 | 2.34 | 29 | 0.345 |
| 3/0 | 9.45 | 14 | 2.03 | 30 | 0.315 |
| 2/0 | 8.84 | 15 | 1.83 | 31 | 0.295 |
| 0 | 8.23 | 16 | 1.63 | 32 | 0.274 |
| 1 | 7.62 | 17 | 1.42 | 33 | 0.254 |
| 2 | 7.01 | 18 | 1.22 | 34 | 0.234 |
| 3 | 6.40 | 19 | 1.02 | 35 | 0.213 |
| 4 | 5.89 | 20 | 0.914 | 36 | 0.193 |
| 5 | 5.38 | 21 | 0.813 | 37 | 0.173 |
| 6 | 4.88 | 22 | 0.711 | 38 | 0.152 |
| 7 | 4.47 | 23 | 0.610 | 39 | 0.132 |
| 8 | 4.06 | 24 | 0.559 | 40 | 0.122 |
| 9 | 3.66 | 25 | 0.508 |
Metric wire for house and workshop circuits
From Wiring and Electrical Safety, for copper wire with home-made covering (varnished cotton or wax) in open air. Bundled, buried or hot wire must be thicker; iron wire of the same size takes no more than a third of these currents.
| Copper cross-section | Diameter | Safe current | Typical use |
|---|---|---|---|
| 0.75 mm² | 1.0 mm | 5 A | Lamp cords |
| 1.5 mm² | 1.4 mm | 10 A | Lighting circuits |
| 2.5 mm² | 1.8 mm | 15 A | Sockets, small motors |
| 4 mm² | 2.3 mm | 20 A | Workshop circuits |
| 6 mm² | 2.8 mm | 30 A | Main feed from the generator |
| 10 mm² | 3.6 mm | 45 A | Large mains |
Sheet metal gauges
Sheet steel in American books is given in the Manufacturers' Standard Gauge; British books use SWG. The two are close in the middle and differ at the ends. Galvanised steel, aluminium and copper sheet use yet other gauges, so measure. Modern sheet is sold in millimetres: common thicknesses are 0.5, 0.6, 0.8, 1.0, 1.2, 1.5, 2.0, 2.5 and 3.0 mm. What thickness to use for each job is in Sheet Metal and Rolling.
| Gauge | US steel sheet (mm) | British SWG (mm) |
|---|---|---|
| 3 | 6.07 | 6.40 |
| 4 | 5.69 | 5.89 |
| 5 | 5.31 | 5.38 |
| 6 | 4.94 | 4.88 |
| 7 | 4.55 | 4.47 |
| 8 | 4.18 | 4.06 |
| 9 | 3.80 | 3.66 |
| 10 | 3.42 | 3.25 |
| 11 | 3.04 | 2.95 |
| 12 | 2.66 | 2.64 |
| 13 | 2.28 | 2.34 |
| 14 | 1.90 | 2.03 |
| 15 | 1.71 | 1.83 |
| 16 | 1.52 | 1.63 |
| 17 | 1.37 | 1.42 |
| 18 | 1.21 | 1.22 |
| 19 | 1.06 | 1.02 |
| 20 | 0.91 | 0.91 |
| 21 | 0.84 | 0.81 |
| 22 | 0.76 | 0.71 |
| 23 | 0.68 | 0.61 |
| 24 | 0.61 | 0.56 |
| 25 | 0.53 | 0.51 |
| 26 | 0.45 | 0.46 |
| 27 | 0.42 | 0.42 |
| 28 | 0.38 | 0.38 |
| 29 | 0.34 | 0.35 |
| 30 | 0.30 | 0.31 |
Screw threads
ISO metric threads
The world standard, with a 60° thread angle. Use the coarse pitch unless you have a reason not to; fine pitches hold better against vibration and in thin walls. Tap drill = major diameter − pitch (Screws, Nuts and Bolts). "Across flats" is the spanner size for an ordinary hexagon nut and bolt head (some older European bolts use 17, 19 and 22 mm for M10, M12 and M14). To check a pitch, measure the length of 10 threads.
| Size | Coarse pitch (mm) | Tap drill, coarse (mm) | Core (minor) diameter of bolt (mm) | Common fine pitch (mm) | Tap drill, fine (mm) | Spanner across flats (mm) |
|---|---|---|---|---|---|---|
| M1.6 | 0.35 | 1.25 | 1.17 | — | — | 3.2 |
| M2 | 0.4 | 1.6 | 1.51 | — | — | 4 |
| M2.5 | 0.45 | 2.05 | 1.95 | — | — | 5 |
| M3 | 0.5 | 2.5 | 2.39 | — | — | 5.5 |
| M4 | 0.7 | 3.3 | 3.14 | — | — | 7 |
| M5 | 0.8 | 4.2 | 4.02 | — | — | 8 |
| M6 | 1 | 5 | 4.77 | — | — | 10 |
| M8 | 1.25 | 6.75 | 6.47 | 1 | 7 | 13 |
| M10 | 1.5 | 8.5 | 8.16 | 1.25 | 8.75 | 16 |
| M12 | 1.75 | 10.25 | 9.85 | 1.5 | 10.5 | 18 |
| M14 | 2 | 12 | 11.55 | 1.5 | 12.5 | 21 |
| M16 | 2 | 14 | 13.55 | 1.5 | 14.5 | 24 |
| M18 | 2.5 | 15.5 | 14.93 | 1.5 | 16.5 | 27 |
| M20 | 2.5 | 17.5 | 16.93 | 1.5 | 18.5 | 30 |
| M22 | 2.5 | 19.5 | 18.93 | 1.5 | 20.5 | 34 |
| M24 | 3 | 21 | 20.32 | 2 | 22 | 36 |
| M27 | 3 | 24 | 23.32 | 2 | 25 | 41 |
| M30 | 3.5 | 26.5 | 25.71 | 2 | 28 | 46 |
| M36 | 4 | 32 | 31.09 | 3 | 33 | 55 |
Inch threads found in salvage
American UNC (Unified Coarse, 60°) and British BSW (British Standard Whitworth, 55°, rounded crests and roots). They are not interchangeable even where the threads per inch match: the angles differ, and a UNC nut on a BSW bolt holds poorly. Count the threads in 25.4 mm (one inch) to identify them.
| Size (inch) | Diameter (mm) | UNC threads per inch (60°) | BSW threads per inch (55°) | UNC pitch (mm) | BSW pitch (mm) |
|---|---|---|---|---|---|
| 1/4 | 6.35 | 20 | 20 | 1.27 | 1.27 |
| 5/16 | 7.94 | 18 | 18 | 1.41 | 1.41 |
| 3/8 | 9.53 | 16 | 16 | 1.59 | 1.59 |
| 7/16 | 11.11 | 14 | 14 | 1.81 | 1.81 |
| 1/2 | 12.70 | 13 | 12 | 1.95 | 2.12 |
| 5/8 | 15.88 | 11 | 11 | 2.31 | 2.31 |
| 3/4 | 19.05 | 10 | 10 | 2.54 | 2.54 |
| 7/8 | 22.23 | 9 | 9 | 2.82 | 2.82 |
| 1 | 25.40 | 8 | 8 | 3.18 | 3.18 |
Dilution tables
Danger Always pour acid into water, never water into acid. Pour slowly, stirring, into a larger volume of cold water in a vessel that can take heat. Wear eye protection. If acid, lye or lime splashes on skin or in the eyes, brush off any dry powder and flood with clean water for at least 20 minutes — for lye or lime in the eye, 30 minutes or more (Emergencies). Do not try to neutralise a chemical burn on the body.
Danger Never mix bleach with acids, vinegar or ammonia (urine). They give off chlorine or other choking gases that can kill. Mix and use bleach in moving air (Chlorine and Bleach).
The rule for any dilution: strength you want × amount you want = strength you have × amount of it you need. Top up with water to the amount you want. Mixing by weight on a balance (Measurement from Scratch) is more exact than by volume for acids, because strong acids are much heavier than water.
Acids: judging strength by weight
Fill the same small cup to the same mark with water, then with the acid, and weigh both. From Sulfuric Acid, Nitric Acid and Hydrochloric Acid.
| A cup that holds 100 g of water holds… | Sulfuric acid | Nitric acid | Hydrochloric acid |
|---|---|---|---|
| about 105 g | — | — | about 10 % |
| about 110 g | — | — | about 20 % |
| about 112 g | about 18 % | — | — |
| about 115 g | — | — | about 30 % (stock acid) |
| about 118 g | — | about 30 % | about 36 % (strongest practical; fumes) |
| about 126 g | about 35 % (battery acid) | — | — |
| about 131 g | — | about 50 % | — |
| about 141 g | — | about 68 % (ordinary concentrated) | — |
| about 150 g | — | about 95 % (fuming) | — |
| about 155 g | about 65 % | — | — |
| about 184 g | about 98 % (concentrated) | — | — |
Acids: mixing a given strength by weight
Weigh the water into the vessel first, then add the weighed acid slowly to it. To turn grams of acid into millilitres, divide by the density: 98 % sulfuric 1.84, 68 % nitric 1.41, 30 % hydrochloric 1.15.
| To make 100 g of… | from 98 % sulfuric acid | from 68 % nitric acid | from 30 % hydrochloric acid |
|---|---|---|---|
| 5 % | 5.1 g acid into 94.9 g water | 7.4 g acid into 92.6 g water | 16.7 g acid into 83.3 g water |
| 10 % | 10.2 g acid into 89.8 g water | 14.7 g acid into 85.3 g water | 33.3 g acid into 66.7 g water |
| 20 % | 20.4 g acid into 79.6 g water | 29.4 g acid into 70.6 g water | 66.7 g acid into 33.3 g water |
| 30 % | 30.6 g acid into 69.4 g water | 44.1 g acid into 55.9 g water | — |
Acid dilutions used in this book
| Job | Mix | Chapter |
|---|---|---|
| Battery acid from concentrated sulfuric acid | About 1 part acid poured into 3 parts water, by volume; fully charged cells read 1.25–1.28 on a hydrometer, flat cells 1.12–1.15 | Sulfuric Acid, The Rechargeable Battery |
| About 10 % sulfuric acid | About 90 g of strong acid poured into 800 mL of water | Hydrogen Peroxide and Oxygen Bleach |
| Pickling iron in hydrochloric acid (about 10 %) | 1 part of 30 % acid into 2 parts water | Hydrochloric Acid |
| Dissolving bone for gelatin (about 5 %) | 1 part of 30 % acid into 5 parts water | Hydrochloric Acid |
| Testing a strong acid's strength | 1 part acid into 9 parts water, then titrate | Acids, Bases and Testing |
| Etching copper with nitric acid | 1 part of 68 % acid into 2–3 parts water | Nitric Acid |
| Etching zinc with nitric acid | 1 part of 68 % acid into 8 parts water | Nitric Acid |
| Etching steel with nitric acid | About 1 part acid into 20 parts water | Nitric Acid |
| Etching copper boards | 2 parts 3 % hydrogen peroxide to 1 part strong hydrochloric acid, outdoors | Hydrogen Peroxide and Oxygen Bleach |
Bleach for drinking water
Use clear water: let muddy water settle or filter it first. These doses are from Chlorine and Bleach; the jar test there finds the right dose for your bleach and your water, and is better than any table.
| Bleach strength | Per litre of water | Per 20-litre bucket |
|---|---|---|
| 0.5 % (homemade by electrolysis) | 8–16 drops (0.4–0.8 mL) | 8–16 mL — about 2–3 teaspoons |
| 1 % | 4–8 drops | 4–8 mL — 1–1½ teaspoons |
| 5 % (old household bleach) | 1–2 drops | ¾–1½ mL — about 15–30 drops |
| Bleaching powder stock (15 g in 1 litre, settled; use the clear liquid) | 8–16 drops | as for 0.5 % |
These give about 2–4 mg of chlorine per litre. Stir, cover, and wait at least 30 minutes — an hour if the water is below 10 °C. It should then have a faint smell of chlorine; if not, add the same dose again and wait 15 minutes more. Use within a day or two. Chlorine does not kill some parasites, such as Cryptosporidium, and does nothing about poisons; when in doubt, boil the water for a full rolling minute (3 minutes above about 2,000 m) (Finding and Purifying Water).
Larger supplies (Water Treatment for a Town, Wells and Cisterns):
| Job | Figure |
|---|---|
| Town supply, filtered water | Usually needs 1–3 mg/L; aim for about 0.5 mg/L left after 30 minutes at the works and at least 0.2 mg/L at the farthest tap |
| Daily chlorine for 100 m³ at 2 mg/L | 200 g of chlorine: 40 L of 0.5 % bleach, 4 L of 5 % bleach, or 0.6–0.8 kg of bleaching powder |
| Shock-dosing a well after cleaning | About 1 L of 5 % bleach per 1,000 L of water in the well (about 50 mg/L); leave 12–24 hours, then draw off until the smell has gone |
Bleach for cleaning and disinfecting
From Chlorine and Bleach. Clean off dirt first; bleach does little under filth.
| Strength | How to make it from 0.5 % bleach | Use |
|---|---|---|
| 0.05 % | 1 part bleach to 9 parts water | Washing hands when soap is scarce, rinsing dishes, soaking clothes of the sick |
| 0.1–0.2 % | 1 part bleach to 3 parts water | Soaking cloth for bleaching, 2–6 hours |
| 0.2 % | 2 parts bleach to 3 parts water | Floors, beds, latrine seats, buckets and tools; leave wet 10 minutes, then rinse |
| 0.5 % (full strength) | as made | Poured on vomit and diarrhoea before cleaning it up |
From 5 % bleach, use one-tenth as much bleach: 0.05 % is 1 part 5 % bleach in 100 parts of mixture (1 + 99).
Hydrogen peroxide
From Hydrogen Peroxide and Oxygen Bleach. "Volume" strength is the litres of oxygen gas one litre gives off.
| Strength | Volume strength | Use |
|---|---|---|
| 1.5 % (3 % mixed 1 : 1 with water) | 5 vol | Mouth rinse, gargle; never swallow |
| 3 % | 10 vol | Cleaning a dirty wound once; ear wax; surfaces |
| 6 % | 20 vol | Bleaching wool, silk, bone; hair |
| 9–12 % | 30–40 vol | Strongest bleaching; burns skin |
| about 30 % | about 100 vol | Laboratory reagent only — the ceiling of this book |
Salt, sugar and lime solutions
| Solution | Recipe | Chapter |
|---|---|---|
| Oral rehydration solution (ORS) | 6 level teaspoons of sugar and ½ level teaspoon of salt in 1 litre of boiled, cooled water; no saltier than tears. Throw away after 24 hours | Oral Rehydration |
| Sea water | About 3.5 % salt | Salt |
| Brine for making bleach | 30 g salt per litre | Chlorine and Bleach |
| Sauerkraut | 20–25 g salt per kg of shredded cabbage (2–2½ %); top-up brine 20 g per litre | Preserving Food |
| Whole fermented vegetables | 35–50 g salt per litre | Preserving Food |
| Brine for pickled onions | 100 g salt per litre, 24 hours, then into vinegar | Vinegar and Pickling |
| Curing brine | 1 kg salt in 4 litres of water (about 20 %); a fresh egg floats with a coin-sized patch showing | Preserving Food |
| Dry-curing meat | At least 50–60 g salt per kg of meat; fish about 1 part salt to 3 parts fish | Preserving Food |
| Curing salts | Never more than 2 g of saltpeter or 2.5 g of curing salt per kg of meat | Sausages, Ham and Bacon |
| Liquid rennet | About 50 g salt per litre (5 %) | Dairy and Cheese |
| Pickling vinegar | At least 5 % acid | Vinegar and Pickling |
| Light syrup for canning fruit | About 200 g sugar per litre of water | Canning and Bottling |
| Limewater for storing eggs | About 30 g slaked lime per litre of boiled, cooled water; use the clear liquid | Poultry and Eggs |
| Soap-strength lye | A fresh egg or small potato floats with a patch 2–3 cm across showing | Lye and Potash |
| Alum for clearing water | Make 1 % (10 g per litre); each 1 mL in 1 litre of raw water gives 10 mg/L; most rivers need 10–50 mg/L | Water Treatment for a Town |
Warning Curing salts are poisons in excess. A few grams of pure sodium nitrite has killed adults. Weigh every time, store cure where it cannot be mistaken for salt or sugar, and never give cured meats to babies under one year (Sausages, Ham and Bacon).
Food storage times
How long food keeps when it was prepared and stored as its chapter describes. Times are a guide, not a promise: throw out anything bulging, spurting, slimy or smelling wrong, without tasting it (Preserving Food).
| Food | How stored | Keeps | Chapter |
|---|---|---|---|
| Milk, fresh | Cool | About a day; spoils within a day in warm weather | Dairy and Cheese |
| Fresh sausage | 1–5 °C | Cook within 2 days; hot-smoked, up to a week in the cold | Sausages, Ham and Bacon |
| Hot-smoked meat or fish | Cool | About a week, unless dried hard | Preserving Food |
| Butter, unsalted | Cool | A week or two | Dairy and Cheese |
| Butter, salted, packed in a crock under brine | Cellar | Months | Dairy and Cheese |
| Ghee | No cooling needed | Months | Dairy and Cheese |
| Hard cheese | Aged at 10–13 °C | Two months to a year of ageing, and keeps about a year | Dairy and Cheese |
| Eggs, unwashed | Warm room / cool cellar under 10 °C | 2–3 weeks / 2–3 months | Poultry and Eggs |
| Eggs in limewater or water glass | Cool, covered | 6–9 months | Poultry and Eggs |
| Eggs, greased and packed in sand, ash or salt | Cool | A few months | Poultry and Eggs |
| Pickled eggs | Below 5 °C | Eat within 3 months | Vinegar and Pickling |
| Vegetables in a clay evaporative cooler | Hot dry climate | 2–3 weeks, against 2–3 days without; not for meat beyond a day or two | Ice and Refrigeration |
| Bacon, cold-smoked | Cool, dry, dark larder | 4–8 weeks | Sausages, Ham and Bacon |
| Sauerkraut | Cool | Months | Preserving Food |
| Pickled red cabbage / pickled onions | Jars of vinegar | 2–3 months / crisp for 6 months | Vinegar and Pickling |
| Cold-smoked, salted fish and ham | Cool, airy | Months | Preserving Food |
| Dry-cured ham | Cool, airy, dark | Aged 6–12 months, until it has lost at least a quarter of its weight | Sausages, Ham and Bacon |
| Jam and other fruit in heavy sugar | Sealed | A year or more | Sugar |
| Chutney | Unopened, cool, dark | 1–2 years | Vinegar and Pickling |
| Canned food in glass jars or tins | Cellar | 1–2 years | Canning and Bottling |
| Grain dried below 13–14 % water | Sealed or a good granary | A year or more; 2–3 years kept well | Granaries and Food Storage |
| Dried yoghurt balls (kurut) | Dry | A year | Dairy and Cheese |
| Pemmican | Cool, dry | Years | Preserving Food |
| Dried cod (stockfish) | Dry | Years | Preserving Food |
| Sugar | Dry | Years | Sugar |
| Vinegar | Full bottles, cool | Years | Vinegar and Pickling |
| Honey | Sealed | Almost forever. Never give to a baby under one year | Beekeeping |
Safety rules that go with these times (Canning and Bottling, Preserving Food):
- Low-acid foods — meat, fish, beans, vegetables, soups — must be pressure canned at 116–121 °C. Boiling-water canning is only for acid foods such as fruit, pickles and acidified tomatoes.
- As an extra safeguard, boil home-canned or other preserved low-acid food hard for 10 minutes before eating; this destroys botulism toxin, though not the spores.
- Cook pork from farmed pigs to 71 °C in the centre and game (bear, boar, walrus and others) to 74 °C. Freezing does not make game meat safe (Sausages, Ham and Bacon).
- Below about 5 °C almost all spoiling microbes slow nearly to a stop; below −18 °C they stop growing, but freezing does not kill them, so thawed food spoils as fast as fresh (Ice and Refrigeration).
- Throw away ORS after 24 hours, cereal ORS after 6–8 hours (Oral Rehydration).
Energy in fuels and foods
Higher figures include the heat in the water vapour from burning, which stoves and engines usually lose. Where a range is given, the low end is what you get in practice. 1 MJ = 0.278 kWh = 239 kcal (Units, Conversions and Mathematical Tables).
| Fuel | Energy per kg | Energy per litre or m³ | Chapter |
|---|---|---|---|
| Green wood (50 % water) | about 8 MJ | — | Firewood and Coppicing |
| Seasoned wood (20 % water) | about 15 MJ | — | Firewood and Coppicing |
| Oven-dry wood | 18–20 MJ | — | Firewood and Coppicing |
| Straw, dried dung | about 12–15 MJ air-dry | — | Biogas and Wood Gas |
| Peat, dry | 14–16 MJ | — | Coal and Coke |
| Lignite (brown coal) | 10–20 MJ | — | Coal and Coke |
| Bituminous coal | 25–33 MJ | — | Coal and Coke |
| Anthracite | 30–33 MJ | — | Coal and Coke |
| Charcoal | 28–31 MJ | — | Charcoal |
| Ethanol | 27–30 MJ | 21–23 MJ per litre | Distillation |
| Plant oil, animal fat | about 37 MJ | about 34 MJ per litre | Oils and Pressing |
| Petroleum, crude | 42–45 MJ | — | Petroleum and Refining |
| Kerosene, diesel, petrol | 43–46 MJ | kerosene and diesel about 35–38 MJ per litre; petrol about 32–35 | Petroleum and Refining |
| Hydrogen | 120–142 MJ | 11–13 MJ per m³ — light, so little per volume | Hydrogen, Oxygen and Gases |
| Natural gas (methane) | — | 35–38 MJ per m³ — about a litre of kerosene | Natural Gas and Helium |
| Biogas (60 % methane) | — | 20–25 MJ per m³ | Biogas and Wood Gas |
| Town (coal) gas | — | 17–20 MJ per m³ | Gas Engines and Producer Gas |
| Producer gas, from wood or coal | — | 4.5–6 MJ per m³ | Gas Engines and Producer Gas |
Food energy (Nutrition and Deficiency Diseases):
| Food part | Energy per gram |
|---|---|
| Carbohydrate (starch, sugar) | 4 kcal (17 kJ) |
| Protein | 4 kcal (17 kJ) |
| Fat | 9 kcal (37 kJ) |
| Alcohol | 7 kcal (29 kJ) |
| Grain, whole | about 3,400 kcal per kg (Grain, Flour and Bread) |
| Pemmican | about 6 kcal per gram (Preserving Food) |
Plan on about 2,100 kcal per person per day on average, more for heavy work, cold or pregnancy (Nutrition and Deficiency Diseases).
Old and common chemical names
Salvaged books, recipes and labels often use these names.
| Old or common name | What it is | Formula | Chapter |
|---|---|---|---|
| Quicklime, burnt lime | Calcium oxide | CaO | Lime |
| Slaked lime, hydrated lime | Calcium hydroxide | Ca(OH)₂ | Lime |
| Limestone, chalk, whiting | Calcium carbonate | CaCO₃ | Lime |
| Gypsum / plaster of Paris | Calcium sulfate with water / with half the water | CaSO₄·2H₂O / CaSO₄·½H₂O | Gypsum and Plaster of Paris |
| Soda ash; washing soda (crystals) | Sodium carbonate | Na₂CO₃; Na₂CO₃·10H₂O | Soda Ash and Baking Soda |
| Baking soda | Sodium bicarbonate | NaHCO₃ | Soda Ash and Baking Soda |
| Caustic soda, lye | Sodium hydroxide | NaOH | Lye and Potash |
| Potash, pearl ash | Potassium carbonate | K₂CO₃ | Lye and Potash |
| Caustic potash | Potassium hydroxide | KOH | Lye and Potash |
| Saltpeter, nitre | Potassium nitrate | KNO₃ | Saltpeter |
| Common salt | Sodium chloride | NaCl | Salt |
| Sal ammoniac | Ammonium chloride | NH₄Cl | Soldering and Brazing |
| Spirit of hartshorn, ammonia water | Ammonia in water | NH₃ | Ammonia |
| Oil of vitriol | Sulfuric acid | H₂SO₄ | Sulfuric Acid |
| Spirit of salt, muriatic acid | Hydrochloric acid | HCl | Hydrochloric Acid |
| Aqua fortis | Nitric acid | HNO₃ | Nitric Acid |
| Aqua regia | 1 part nitric to 3 parts hydrochloric acid; dissolves gold | — | Gold and Silver |
| Green vitriol, copperas | Iron(II) sulfate | FeSO₄·7H₂O | Sulfuric Acid, Ink |
| Blue vitriol, bluestone | Copper sulfate | CuSO₄·5H₂O | Copper Smelting |
| White vitriol | Zinc sulfate | ZnSO₄·7H₂O | Zinc and Brass |
| Epsom salt | Magnesium sulfate | MgSO₄·7H₂O | Magnesium |
| Glauber's salt | Sodium sulfate | Na₂SO₄·10H₂O | Soda Ash and Baking Soda |
| Alum | Potassium aluminium sulfate | KAl(SO₄)₂·12H₂O | Alum and Alumina |
| Borax | Sodium borate | Na₂B₄O₇·10H₂O | Borax and Boric Acid |
| Water glass | Sodium silicate | Na₂SiO₃ and similar | Water Glass (Sodium Silicate) |
| Chloride of lime, bleaching powder | Calcium hypochlorite with lime | — | Chlorine and Bleach |
| Hypo | Sodium thiosulfate | Na₂S₂O₃·5H₂O | Photography |
| Lunar caustic | Silver nitrate | AgNO₃ | Silver Nitrate and Silver Salts |
| Cream of tartar | Potassium hydrogen tartrate | KC₄H₅O₆ | Citric and Tartaric Acid |
| Litharge / red lead / white lead | Lead oxide / lead tetroxide / lead carbonate — all poison | PbO / Pb₃O₄ / 2PbCO₃·Pb(OH)₂ | Lead, Pigments, Paints and Varnish |
| Verdigris | Copper acetate or carbonate (green rust of copper) | — | Pigments, Paints and Varnish |
| Corrosive sublimate | Mercury(II) chloride — deadly poison | HgCl₂ | Mercury |
| Wood spirit | Methanol — poison | CH₃OH | Distillation |
| Spirit of wine | Ethanol | C₂H₅OH | Distillation |
| Oil of turpentine | Turpentine | — | Tar, Pitch and Glue |
| Galena | Lead sulfide (lead ore) | PbS | Lead |
| Cassiterite, tinstone | Tin oxide (tin ore) | SnO₂ | Tin and Pewter |
| Hematite / magnetite | Iron oxides (iron ores) | Fe₂O₃ / Fe₃O₄ | Finding and Identifying Ores |
| Pyrite, fool's gold | Iron sulfide | FeS₂ | Sulfur |
| Malachite | Copper carbonate (copper ore) | Cu₂CO₃(OH)₂ | Copper Smelting |
| Cinnabar | Mercury sulfide (mercury ore) — poison | HgS | Mercury |