◆ Rebuild

Part 2 · Earth and Fire

Tiles and Clay Pipes

How to make fired clay roof tiles that keep out rain and fire for a century, floor tiles that give a clean, dry floor, and clay pipes that drain fields, carry water and take away sewage — with simple moulds, formers and a hand press, and how to join and lay them.

Difficulty
●●●●●
Time
A day to make 100–200 tiles or 30–60 pipes; two to four weeks to dry; a firing to finish
Steps from zero
4 prerequisites →

You need first

PotteryThe Kiln

This unlocks

Pipes, Plumbing and AqueductsRoofsLaying Tiles and Mosaics
The full path from nothing — 4 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery
  4. The Kiln
  5. Tiles and Clay Pipes

Do them roughly in this order. See it on the tech tree →

Why it matters

Thatch and bark roofs rot, leak and burn. A fired clay tile roof lasts 50 to 100 years or more, does not burn, and gives clean rainwater for a cistern (see Wells and Cisterns). In a town, it stops a single kitchen fire from burning down a whole street.

Floor tiles turn a dusty or muddy earth floor into one that can be swept and washed, which keeps out fleas, worms and damp (see Sanitation and Germs and Foundations and Floors).

Clay pipes carry water where you want it and take it away from where you don't:

How it works

Tiles and pipes are Pottery with special shapes. They face two problems that ordinary pots do not:

  1. Warping. Thin, flat or long pieces dry unevenly and twist. The cure is a well-tempered clay, even thickness, slow drying, and drying on or in a former that holds the shape.
  2. Weather. Roof tiles and buried pipes stay wet for months. Water soaks into the pores; when it freezes it expands by about a tenth and splits the clay. Tiles must be fired hot — at least 950–1,050 °C (orange heat), so that they absorb little water — and made from a clay without lime lumps (see Finding and Preparing Clay).

Roof tiles shed water by overlapping. Every gap between two tiles is covered by another tile above or across it. The steeper the roof, the less overlap is needed and the faster rain runs off. Flat tiles need a steep roof; curved tiles that form channels work on gentler slopes.

Pipes join by a spigot and socket. Each pipe has a plain end (the spigot) and a widened end (the socket, or bell). The spigot of one pipe slides into the socket of the next, and the ring-shaped gap between them is packed with a seal.

What you need

Item Notes
Clay, tempered Pottery clay with 20–30% sand or grog (see Finding and Preparing Clay); a lean, sandy clay warps less
Moulding table A flat, sturdy board or slab, dusted with fine sand
Frame moulds Thin wooden frames the shape of the tile; see below
Formers Smooth tapered wooden blocks or log halves for curved tiles; round tapered wooden rods (mandrels) for pipes
Cutting wire or thin blade, a straightedge For trimming
Drying racks Shelves under a roof, out of sun and wind
Kiln A The Kiln or brick clamp (see Bricks) able to reach orange heat
For jointing pipes Hemp or flax fibre, lime mortar (see Lime and Mortar and Concrete), or pitch (see Tar, Pitch and Glue)

The tile types

Barrel tiles (end view) Roman tiles (end view) Plain tiles on battens (side view, roof sloping down to the right) channel: carries the rain cap: covers the gap tegula: flat, with raised edges imbrex: half-round cover nib hooks over the batten each joint is covered by two layers batten, about 10 cm gauge
Fig. 1 Three kinds of roof tile and how they overlap. Plain tiles hang from battens by nibs and overlap twice; barrel tiles lie in channels and caps; Roman tiles use a flat flanged tile with a half-round cover over each joint.
Tile Shape and size Roof slope Tiles per m² Notes
Barrel tile (Spanish, mission) Tapered half-cylinder, about 45 cm long, 20 cm wide at one end and 15 cm at the other, 1.5 cm thick 20–35° About 25–30 Easiest to make; laid in rows of channels (concave up) and caps (convex up)
Roman tile (tegula and imbrex) Flat tile with raised edges about 50 × 40 cm, plus a half-round cover tile over each joint 15–30° About 6–8 flat + covers Heavy but very weatherproof
Plain tile Flat, 26 × 16 cm, 1.2 cm thick, with two nibs (little hooks) on the back of the top edge and nail holes 40–60° About 60 Hangs on wooden battens; needs a steep roof and a good wooden frame

A tiled roof is heavy — about 50–80 kg per square metre, five to ten times as heavy as thatch. The rafters and walls must be built for it (see Roofs and Timber Framing and Log Building).

Step by step: barrel tiles

  1. Make a frame mould: a flat wooden frame 1.5 cm deep, cut to the outline of the flattened tile — a long trapezium about 45 cm long, 22 cm wide at one end and 17 cm at the other.
  2. Make a former: a smooth wooden block shaped like a half-cone the size of the inside of the finished tile, with a handle. A split log tapered with an adze works well.
  3. Mould the slab. Set the frame on the sanded table, throw in a lump of well-wedged clay hard enough to fill it, press it into the corners, and cut off the surplus with a wet straightedge or a wire drawn across the top of the frame.
  4. Bend it. Lift the frame off. Sand the former, slide the slab onto it (or lift the slab on a cloth and lay it over), and smooth it down with wet hands so it takes the shape.
  5. Turn it out onto a sanded drying board, standing on its edges, and slide out the former. Make the next one.
  6. Dry slowly in shade for two to three weeks. Turn tiles end for end after a few days so they dry evenly.

A practised pair of tile-makers can make several hundred a day this way.

Step by step: plain and floor tiles

  1. Frame mould 1.2 cm deep for roof tiles, 2–2.5 cm deep for floor tiles. Floor tiles are commonly 20 × 20 cm or 25 × 25 cm.
  2. Fill, strike off, and lift the frame as above.
  3. Roof tiles: while soft, pinch up two nibs on the back at the top edge (or press in two lumps of clay and smooth them on), and push two nail holes through with a stick.
  4. Lay flat to dry on a sanded board. Put a second sanded board on top after the first day, with a light weight, to stop curling. Turn them over every day or two.
  5. For floor tiles that must be truly flat, beat them when leather-hard: lay each on a flat board and tap it all over with a flat wooden paddle, then trim the edges square with a knife against a wooden square.
  6. Dry for two to four weeks before firing.

Step by step: clay pipes

1. Wrap a slab round a cloth-covered mandrel 2. Joint in cross-section: spigot in socket Socket collar2–3 cm wider than the spigot Slab 1.5–2 cm thickseam scored, slipped, smoothed cloth so it slides out Tapered wooden mandrel60–70 cm long hemp packing lime mortar, bevelled spigot of next pipe Downhillsocket faces uphill; water flows from spigot into socket Uphill
Fig. 2 Making a pipe on a mandrel. A clay slab is wrapped round a tapered wooden rod covered with cloth and joined with a scored seam; a thickened collar forms the socket. Below: two pipes joined, the spigot in the socket and the gap packed with fibre and mortar.

By hand on a mandrel

  1. Make the mandrel: a smooth, straight wooden rod 60–70 cm long, very slightly tapered (1 cm narrower at one end) so it slides out. For a pipe of 10 cm inside diameter, the rod is 10 cm across. Wrap it in a single layer of cloth or dust it with fine sand so clay does not stick.
  2. Roll a slab 1.5–2 cm thick and as long as the pipe (40–60 cm is a good length) and as wide as the mandrel's circumference plus 3 cm.
  3. Wrap it round the mandrel. Cut the overlapping edges at a slant, score both with a stick, wet them with slip, press them together, and smooth the seam inside and out until it vanishes.
  4. Form the socket. At one end, wrap an extra band of clay 6–8 cm wide around the pipe, or slide on a short, wider collar made on a fatter rod. The socket's inside must be about 2–3 cm wider than the outside of the spigot, to leave room for the seal.
  5. Stand it up on its socket on a sanded board and draw out the mandrel. Leave the cloth in until the clay stiffens, then peel it out.
  6. Dry standing upright, slowly, for two to three weeks. Pipes dried lying down sag into ovals.

Pipes can also be thrown on a potter's wheel (The Potter's Wheel) in sections, as the Romans did, or made in two halves in a mould and joined.

Field drain tiles

For land drains, simpler pipes do: plain tubes 30–35 cm long and 5–8 cm across, with no socket. They are laid end to end in a trench, touching, and water seeps in through the joints. Older drains used horseshoe tiles — half-pipes laid over a flat sole tile.

Extruding with a press

A pipe press pushes stiff clay through a die, giving a continuous pipe that is cut to length. It is a strong box or cylinder, with a ring-shaped opening at the bottom: an outer ring (the die) with a central round core held in place by a thin cross-bar (the bridge). A plunger, driven down by a big screw or a long lever, pushes clay through; the clay splits around the bridge and welds back together below it. Hand-powered presses of the 1840s made thousands of drain pipes a day. Building one needs good Basic Woodworking or iron, and very stiff, well-mixed clay. Make pipes by hand first.

Firing

  • Fire tiles on edge, packed close in a herringbone pattern, so heat passes between them. Floor tiles can stand on edge or be stacked flat with sand between them.
  • Stand pipes upright on their sockets, small ones inside large ones.
  • Fire slowly through the steam stage (see The Kiln) — thick pipes and tightly packed tiles hold water.
  • Fire to orange heat, 950–1,050 °C, and soak for an hour. Underfired tiles crumble with frost in one winter.
  • Tiles and pipes can also be fired in a brick clamp with a load of Bricks.

Laying

Roof tiles. Start at the eaves and work up, so each row overlaps the one below. For barrel tiles, lay the channel tiles (concave up, wide end at the top) side by side with a gap of 5–8 cm, then lay cap tiles (convex up, wide end at the bottom) over the gaps. Each tile overlaps the one below it by at least 8–10 cm. Bed the eaves row and the ridge in lime mortar. Plain tiles hang by their nibs on wooden battens nailed across the rafters; space the battens so each tile covers two others at its tail (about 10 cm "gauge" for 26 cm tiles), and nail every fourth or fifth row.

Floor tiles. Lay on a firm, level bed of dry, rammed earth or gravel covered with 3–5 cm of lime mortar or sand. Soak tiles in water first so they don't suck the water out of the mortar. Leave joints of 3–6 mm and fill them with lime mortar. More on laying and finishing tiled floors and walls is in Laying Tiles and Mosaics.

Pipes.

  1. Dig the trench to an even fall. Field drains go 75–100 cm deep, with a fall of at least 1 in 200 (half a centimetre per metre), better 1 in 100. Water and sewer pipes need a steady, smooth slope with no humps or dips — check it with a water level (see Surveying and Levelling).
  2. Lay from the low end uphill, with each socket facing uphill, so water flows from spigot into socket and never against the joint.
  3. Bed each pipe on 5 cm of sand or fine gravel, scooping a hollow under the socket so the pipe rests on its barrel, not on the socket.
  4. Seal each joint: push the spigot fully home, ram a twist of hemp or flax (tarred, if you have tar) into the bottom of the gap to centre the pipe and stop mortar running in, then fill the rest with stiff lime mortar (or clay mixed with a little lime) and bevel it off. For a joint that can flex a little, fill with hot pitch mixed with sand instead.
  5. Test before burying: block the low end, fill the line with water, and leave it for an hour. Look for wet spots at the joints. Then backfill gently, by hand around the pipes, before shovelling in the rest.

Warning Clay pipes are for gravity flow. Earthenware pipes and mortar joints will burst or leak under the pressure of more than a few metres of water. For water that must climb over hills or run downhill a long way and then up again (an inverted siphon), use pipes of stone, Lead, cast iron, or very carefully made vitrified stoneware (Stoneware and Porcelain), and see Pipes, Plumbing and Aqueducts.

How to tell it worked

  • Tiles and pipes ring clearly when tapped. A dull note means a crack.
  • Soak test: weigh a dry tile, soak it in water for a day, weigh it again. A good roof tile gains less than about a tenth of its weight; less is better.
  • Strength test: lay a dry roof tile across two bricks 20 cm apart and set a 20 kg stone gently on the middle. It should hold.
  • Leak test for pipes: stand a pipe on a plugged socket, fill it with water, and leave it for an hour. The outside may darken; it must not drip.
  • The first winter is the true test of tiles: count the cracked or flaking ones in spring.

Note Troubleshooting. Tiles warp and twist → dried too fast or unevenly; dry under weights, in shade, turning often; add more sand or grog. Tiles crack across while drying → too thin in places, or clay too sticky; add temper, make the slab even. Tiles flake and crumble after frost → underfired, or lime specks in the clay; fire hotter, clean the clay. Pipes sag into ovals → dried lying down, or clay too soft; stand them up and use stiffer clay. Seam splits on pipes → edges not scored and slipped; score, slip and smooth harder. Joints leak → spigot not fully home, no fibre packing, or mortar too wet; also check for a cracked pipe. Drain stops running → silt in the line, a dip where silt collects, or roots; lay to an even fall and keep trees away.

Dangers

Danger Falls from roofs kill. Work on a roof only with a firm ladder tied at the top, a roof ladder or footboards hooked over the ridge, and never on wet or icy tiles. Keep the ground below clear of people — a dropped tile can kill.

Danger Trench collapse. Soil walls can fall without warning and bury a person. Any trench deeper than your waist must have its sides sloped back or shored with planks and props. Never work in a deep trench alone, and keep the spoil heap at least half a metre back from the edge.

  • Roof overload. A tiled roof weighs many tonnes. Never tile a roof framed for thatch without strengthening it.
  • Clean water and dirty water. Lay drinking-water pipes well away from and uphill of sewer pipes, latrines and cesspits, and never in the same trench. A leaking sewer can poison a water line (see Sanitation and Germs).
  • Never use lead-glazed pipes for drinking water (see Glazes).
  • Heavy lifting. Stacks of tiles and pipes are heavy; lift with your legs, carry in pairs.

What this unlocks

Tiles give fireproof, long-lasting Roofs and clean floors. Pipes make possible field drainage for Farming from Seed, gravity water supply and aqueducts (Pipes, Plumbing and Aqueducts), Sewers and Wastewater, and Chimneys, Stoves and Heating. Glazed and vitrified pipes (Glazes, Stoneware and Porcelain) last for centuries underground and resist sewage and acids.

How it was first done

Fired clay pipes were laid in Mesopotamia by about 4000 BC, and the cities of the Indus Valley (about 2500 BC) had covered brick drains along their streets. At the palace of Knossos on Crete (about 1700 BC), tapered terracotta pipes fitted one into the next carried water. The earliest known fired roof tiles come from Greece, from about 2500 BC, and from China by about 1000 BC; the Greeks and Romans roofed whole cities with flat and half-round tiles. Tile drainage of fields spread in Britain in the early 1800s and became cheap in the 1840s, when hand-operated presses began extruding drain pipes by the thousand; in 1838 John Johnston laid the first clay field drains in the United States, in New York. From the 1840s, salt-glazed stoneware sewer pipes were made in London, and they carried the sewers of the world's great cities for the next hundred years.

Source: content/entries/earth/tiles-and-pipes.md