◆ Rebuild

Part 3 · Metals

Scissors, Shears and Folding Knives

Two steel edges that slide past each other cut cloth, hair, wool, paper, twigs and sheet metal far more cleanly than one blade. How spring shears and pivoted scissors are forged, bevelled, set and riveted; how tailor's shears, pruning shears, tin snips and nail scissors differ; how a pocket knife's back spring holds its blade; and how to keep every edge sharp.

Difficulty
●●●●●
Time
A day to forge a pair of spring shears; two to three days for a first pair of pivoted scissors or a pocket knife
Steps from zero
14 prerequisites →

You need first

SteelAxes, Chisels, Knives and PlanesBlacksmithing

This unlocks

—
The full path from nothing — 14 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing
  13. Steel
  14. Axes, Chisels, Knives and Planes
  15. Scissors, Shears and Folding Knives

Do them roughly in this order. See it on the tech tree →

Why it matters

A knife pushes a thin wedge into the material. Soft, loose things — cloth, wool, hair, thread, paper — just move away from it. Shears trap the material between two edges that pass each other, so it cannot escape. They cut cloth along a line for Making Clothes, take a fleece off a sheep without harming it (Wool), trim hair and nails, prune trees (Fruit Trees and Orchards), and cut sheet metal for every can and bucket (Tins, Cans, Drums and Tanks).

The folding knife solves a different problem: a sharp blade you can carry safely in a pocket every day. With its smaller cousins it is the tool people reach for most often.

How it works

Shearing. Two edges close past each other. The material between them is squeezed, then split along the line where the edges meet. Because the edges do not have to wedge anything apart, they can be blunt-angled: scissor edges are ground at 60–85°, where a knife is 30–40°. That is why good scissors stay sharp for years.

Pivoted scissors from above Bows finger rings, left soft shank Pivot rivet or screw, 4–5 mm stop Blade hardened, tempered straw–brown edge: where the blades meet tip The set, seen from the side (curve exaggerated; really 1–1.5 mm) light shows between the blades touch at tip pivot Blades crossing, end-on 70–80° flat inner face cloth
Fig. 1 Anatomy of scissors. Each blade bows slightly toward the other, so the two touch at only one point, which travels from pivot to tip as they close. The edge is a steep bevel; the inner face is flat or very slightly hollow.

The blades must press together at the cutting point. If there is even a hair's gap where the edges cross, cloth folds into it and is chewed, not cut. So:

  • Each blade is bowed very slightly toward the other along its length (the set). Held closed and looked at from the side, light shows between them except at the pivot and the tips.
  • The pivot holds them firmly together, so as they close the bowed blades press at one moving point — and only there. Friction stays low; the pressure stays where the cutting happens.
  • The inner faces are flat or very slightly hollow across their width, so only the edges rub.

The edge angle (between the bevel and the flat inner face) suits the job:

Tool Edge angle
Hair and fine embroidery scissors 55–65°
Household and tailor's scissors 70–80°
Sheep shears 65–75°
Tin snips 80–85°

Leverage. The force at the edge is the force on the handles times (handle length ÷ distance from pivot to the cut). Cutting near the pivot is strongest; tin snips have short blades and long handles, about 4:1.

Hardness. Blades must be hard to hold an edge but tough enough not to chip; handles and springs must flex without breaking. You harden the blade and temper it to straw to brown (230–260 °C), and temper springs and bows to blue (about 300 °C), as in Steel.

What you need

Item Notes
Steel Carbon steel for blades and springs (Steel); iron for bows and handles, with steel edges welded on (Axes, Chisels, Knives and Planes)
Forge tools Anvil with a small beak, hammers, tongs, punches, drift (Blacksmithing)
Files and stones Flat, half-round and small round files (Files and Saws); sandstone, then a fine whetstone
Rivet wire Soft iron, brass or copper, 2–5 mm (Iron and Brass Wire)
Handle material Horn, bone, antler or close-grained hardwood (Horn and Bone Working)
Liners Brass sheet 0.8–1 mm for pocket knives (Zinc and Brass)
Quench Water or brine for thick parts; oil or melted fat for thin blades

Where to find it

The metal comes from Steel and Iron (the Bloomery). Handle scales come from cattle shin bone (boiled and degreased), horn and deer antler; boxwood, olive, walnut and fruitwoods are the best woods. A fine whetstone — slate or fine sandstone — finishes every edge (Abrasives and Grinding Stones).

Spring shears

The oldest shears are one piece of steel bent into a U: two blades joined by a springy bow. Squeeze them and they close; let go and the bow opens them. They are easier to make than pivoted scissors, need no rivet, and are still the best tool for sheep shearing and for trimming grass and hedges.

Spring shears for sheep one piece of steel; squeeze to close, the bow opens them Bow Blades stop squeeze bow: flat spring 25–30 × 2–2.5 mm, tempered blue handles: soft, rounded to the hand blades: 13–15 cm, hardened, tempered brown; a stop keeps the tips from crossing more than 5 mm 30–33 cm overall Bypass pruning shears cut living branches up to 15–20 mm Blade single bevel, tempered straw Hook soft; holds the branch branch pivot bolt spring opens the handles
Fig. 2 Left: spring sheep shears, one piece of steel; the bow is a flat spring tempered blue. Right: bypass pruning shears; a sharp blade passes close beside a thick hook that holds the branch.

Sheep shears (overall 30–33 cm; blades 13–15 cm long and 3–4 cm wide at the heel):

  1. Forge the bar. Take steel bar about 15 × 8 mm and 50 cm long. Leave about 15 cm at each end thick for the blades and handles; draw the middle 20 cm out into a flat strip 25–30 mm wide and 2–2.5 mm thick — this will be the bow.
  2. Shape the blades. Forge each end into a blade: flat on the inner side, thick at the back (4–5 mm) and thin at the edge (about 1 mm), tapering to a point. Behind each blade, leave a handle part about 10 cm long, rounded to fit the hand.
  3. Bend the bow round a 4–5 cm round bar into a U, so the two blades lie side by side. Then twist each blade a quarter turn at the neck so their flat faces meet and their edges face each other, one above the other. Now they cross like scissors when squeezed.
  4. Grind the inner faces flat and the edge bevels to about 70°.
  5. Harden the blades only: heat the front 10 cm of each to cherry red and quench in oil. Temper the blades brown. Then heat the bow gently and let the colour run to blue, and no further.
  6. Set. Bend the blades gently so they press together at the heel and cross by about 5 mm at the tips when fully closed. A small stop — a lump forged on one handle — keeps them from crossing further.

A good pair opens by itself to about 6–8 cm between the tips, closes with a light squeeze, and cuts a lock of wool cleanly with the very tips. If the bow takes a permanent set after use, it was tempered too soft or is too thin; if it snaps, it was too hard.

Smaller spring shears — 12–15 cm, made the same way from thinner stock — are the best tool for snipping thread at the sewing table (Sewing, Needles and Thread).

Pivoted scissors

Making a pair

For household scissors 15–18 cm long. Make the two halves together and as a matched pair.

  1. Forge each half from steel bar about 12 × 6 mm: a blade 7–9 cm long, 12–15 mm wide at the pivot tapering to the point, thick at the back (3 mm) and thin at the edge; a flat round pivot boss about 15 mm across; and a shank that ends in the bow (finger ring). For the bow, draw the end into a round rod 6–7 mm thick, bend it into a ring over the beak, and weld the end back onto the shank — or flatten the end into a pad, punch a hole and drift it open to a ring 20–25 mm inside.
  2. Bend the shank slightly so that when both blades lie flat together, the bows sit a finger's thickness apart.
  3. File and grind. Grind the inner face of each blade dead flat on a flat stone; then grind it very slightly hollow across its width, so only the edge and the back touch a straightedge. Grind the outer bevel.
  4. Drill or punch the pivot hole through both halves together, clamped in their closed position: 4–5 mm.
  5. Set the bow in each blade while it is still soft: lay it on a block of end-grain wood and tap it so the blade curves 1–1.5 mm toward the other half over its length.
  6. Harden and temper. Heat the blade to cherry red — not the bow — and quench in oil. Polish a spot and temper the blades to dark straw or brown; let the shank and bows run to blue.
  7. Correct the set. Close the blades on the pivot. If the set has changed in quenching, warm the blade to its tempering colour again and bend it gently between padded vice jaws.
  8. Grind the edges to the final angle and lap the inner faces lightly on a fine stone to remove the burr.
  9. Rivet. Put a soft iron or brass rivet through both halves, with a thin washer under the head on each side, and peen it with light blows until the scissors open and close with a firm, even drag. Better still, tap a thread in one half and use a screw, so the tension can be adjusted (Screws, Nuts and Bolts). File a small stop on one shank so the tips cannot cross more than 2–3 mm.

A good pair moves smoothly with no gritty or tight spots; held to the light, a single bright contact point travels from pivot to tip; it cuts a thread or wet paper right at the tips; nothing wobbles at the pivot. A bad pair folds cloth instead of cutting it.

Tailor's shears

Tailor's shears are long (25–30 cm), heavy scissors with blades 12–15 cm long. The lower handle is bent down so the bottom blade slides flat along the table under the cloth without lifting it; the lower bow is large, for two or three fingers, the upper bow small, for the thumb. Forge them as above from heavier stock (16 × 8 mm), or make the handles of iron with steel blades welded on (Axes, Chisels, Knives and Planes). Use a screw pivot. A tailor keeps them for cloth only — paper dulls them (Tailoring and Pattern Drafting).

Nail scissors

Nail scissors are about 9 cm long with blades only 2.5–3 cm, very fine points, and blades curved sideways to follow the curve of a nail. Forge them small from 6 × 4 mm steel; before hardening, bend both blades together round a former of about 3 cm radius. Grind the edges at about 65°, temper straw, and set them very lightly. They must cut a fingernail without twisting it. For nail clippers and other grooming tools, see Razors, Nail Clippers and Grooming Tools.

Pruning shears

Pruning shears (secateurs) cut living branches up to 15–20 mm. In the bypass kind, one sharp blade, bevelled on the outside only, sweeps close past a thick, curved hook that holds the branch so it cannot slide out. The cut is clean and heals well. In the anvil kind, a straight blade closes against a flat pad of brass or soft iron; it cuts dead wood with less effort but crushes living stems.

  1. Blade: steel 4–5 mm thick, 5–6 cm long, curved like a crescent, flat inside, with a single bevel of 25–30° — closer to a knife than a scissor, because it must enter wood.
  2. Hook: iron or steel 6–8 mm thick, curved to meet the blade, with a flat inner face. Leave it soft.
  3. Handles: 15–18 cm long, forged on each part or riveted on.
  4. Pivot: a bolt and nut, 6–8 mm, so you can take up wear (Screws, Nuts and Bolts).
  5. Spring: a coil spring between the handles, or a small leaf spring riveted to one handle and pressing on the other (Springs); and a latch — a wire loop or catch — to hold them closed in the pocket.
  6. Harden the blade and temper it straw; the hook and handles stay soft.

Cut with the blade on the side of the plant that stays, so any crushing is on the piece you discard.

Tin snips

The basics are in Sheet Metal and Rolling. Straight snips for sheet up to about 0.8 mm iron or 1 mm copper: overall 25–30 cm, blades 6–8 cm long and 5–6 mm thick at the back, handles three to four times as long as the blades. Grind the edges at 80–85°, almost square. Harden the blades and temper them brown to purple: harder chips, softer folds over. Curved blades cut circles more easily; compound snips, with a second pivot and link that multiply the force, cut thicker sheet but are harder to make. Thicker sheet goes to the bench shears or chisel.

Folding knives

How the back spring works

A pocket knife (slip-joint knife) has a blade that pivots on a pin between two thin metal plates (liners) inside a handle. Along the back of the handle runs a flat steel back spring, held by a pin near its middle. The spring's front end presses on the blade's tang (the part inside the handle). When the blade is open, it presses on the tang's flat top and holds the blade straight. Turning the blade forces the tang's square corner to lift the spring, so the blade resists and then snaps over; halfway, the spring rests on the squared end of the tang (the half-stop), which keeps a half-open blade from closing on your fingers. Closed, the spring presses on a small bump on the edge side of the tang (the kick), which holds the blade shut and keeps its edge from touching the spring. For this to work, the tang's flat top and its end must be the same distance from the pivot centre.

Open Back spring spring presses on the tang's flat top: holds it open blade centre pin end pin pivot pin Closed spring presses on the kick: holds it shut, edge kept clear spine and nail nick show at the front Sizes closed length 9–10 cm; blade 7–8 cm × 2–2.5 mm, tempered straw spring 2.5–3 mm, tempered blue along its whole length liners 0.8–1 mm brass; pins 2.5–3 mm, peened flush Handle cut across pin, peened spring brass liner closed blade scale
Fig. 3 A slip-joint pocket knife, with the handle drawn as if transparent. Open, the back spring presses on the tang's flat top; closed, it presses on the kick. Right: the handle cut across, showing the layers of scale, liner, spring and blade held by peened pins.

The simplest folding knife

Before spring knives, people carried friction folders: a blade pivoting on a pin through a split wooden or horn handle, with a long tail on the tang (the lever) that lies along the back of the handle when the blade is open. Your fingers hold the lever down while you cut. A ring that turns on the handle to block the blade (the ring lock) makes it safe. Make one first: no spring, no fine fitting.

Making a slip-joint knife

Sizes for a sturdy pocket knife: closed length 9–10 cm, blade 7–8 cm long and 2–2.5 mm thick, spring 2.5–3 mm thick and as long as the handle, liners 0.8–1 mm brass, pins 2.5–3 mm brass or iron wire.

  1. Draw a full-size pattern of the handle, the blade (open and closed) and the spring on thin board. Mark the pivot centre. Fit everything on paper first.
  2. Forge the blade with its tang from carbon steel. File the tang to the pattern: its flat top in line with the spine, its end square to that, both exactly the same distance from the pivot hole, and a small kick on the edge side. Drill the pivot hole. File a nail nick in the blade near its back for opening.
  3. Forge the spring from steel strip, file it to the pattern, and drill holes for its centre pin. Its front end must bear flat on the tang.
  4. Cut two liners of brass to the handle outline and drill the pivot, spring-pin and end-pin holes through both together.
  5. Assemble dry with loose pins. Adjust with a file until the blade snaps firmly open and closed, sits centred between the liners, and the closed edge clears the spring and the bottom of the handle.
  6. Harden the blade (temper straw) and the spring (temper blue, evenly along its whole length — a spring left hard in one spot snaps there).
  7. Fit scales of horn, bone, antler or wood to the liners, drill them, and peen the pins over slightly countersunk holes until the heads are flush. File and polish the edges of the whole handle together.
  8. Sharpen at 15–20° each side (Axes, Chisels, Knives and Planes).

How to tell a good one: the blade "walks" (opens with an even pull) and "talks" (closes with a crisp click); it sits dead centre when closed and does not wobble sideways or up and down when open; the edge never touches the spring.

Locks

A slip joint can fold on your fingers if you push the back of the blade. A lockback prevents it: the spring has a hook near its front that drops into a notch in the tang when the blade opens; to close, you press the rear end of the spring, which pivots on its centre pin and lifts the hook. Make one only after a good slip joint — the hook and notch must fit with no play at all.

Sharpening steels and keeping edges

A sharpening steel is a round or oval rod of very hard steel, 25–30 cm long and 10–13 mm thick, often with fine grooves along its length, a wooden or horn handle and a guard to protect the hand. It does not grind metal away: it straightens an edge that has rolled over in use, which is most of what "blunt" means for a butcher's or kitchen knife.

Making one: forge a round rod from your hardest, highest-carbon steel; draw a tang for the handle. File fine grooves along it 0.3–0.5 mm apart, all the way round, or leave it polished smooth. Harden it fully in water and temper only to pale straw (about 200 °C), so it is harder than any knife it touches. Fit a handle and an iron or brass disc as a guard.

Using it: stand the steel point-down on a board. Lay the knife's heel against the top at 15–20°, and draw it down and back so the whole edge passes along the steel, with light pressure. Alternate sides, 5–10 strokes each. When the steel no longer brings the edge back, it is time for the stone.

Keeping scissors sharp:

  1. Open the scissors fully. Hold a flat fine stone against the outer bevel only, at its original angle, and stroke from pivot to tip until a fine burr forms on the inner side.
  2. Never grind the inner face round or bevel it. At most, lay it flat on the stone and give it one light pass to remove the burr; or simply open and close the scissors a few times.
  3. Tighten the pivot if the blades have worked loose; oil it.
  4. If they still fold cloth, the set has gone: re-bend the blades slightly toward each other.

Snips and shears are sharpened the same way. Knives: grind, hone and strop as in Axes, Chisels, Knives and Planes and Sharpening and Honing.

How to tell it worked

Each section above gives its own test. In general: blades cut a single thread at the tips; against the light, one bright contact point travels from pivot to tip; springs return fully after a thousand squeezes; a file skates on the hardened edge but bites the bows and handles.

Note Troubleshooting. Scissors fold cloth between the blades → too little set, or the pivot is loose. Tighten the pivot; re-bend the blades toward each other. Scissors stiff and grinding → too much set, or a burr on the inner face. Ease the set; lap the inner faces lightly. Edge chips → tempered too hard. Re-temper a shade darker. Edge folds over on sheet metal → too soft, or the angle too thin. Re-harden; grind steeper. Spring shears do not reopen → bow too soft or too thin; re-harden and temper the bow blue, or forge it thicker. Knife blade wobbles → pivot hole too big or pins too loose. Re-peen, or fit a larger pin. Knife blade flops or will not snap → tang top and end not equally far from the pivot, or the spring is too soft. File the longer face; re-harden the spring.

Dangers

Warning A slip-joint blade can close on your fingers. Never push on the back of a non-locking blade; cut away from yourself; close the knife with the palm clear of the edge's path. Children should start with a locking or fixed-blade knife.

Warning Quench oil catches fire. A red-hot blade plunged into too little oil, or oil that has grown hot from many quenches, can flare into flames. Use a lidded metal pot holding at least a few litres, keep it away from the forge, plunge the blade fully in at once, and if it lights, put the lid on — never throw water on burning oil (Steel).

  • Springs can fly out when a part breaks or is being fitted. Protect your eyes.
  • Sheep shearing: the tips can stab the sheep or you. Keep the lower blade flat on the skin and stretch the skin where it folds (Wool).
  • Never test an edge by running a finger along it.

What this unlocks

Shears and scissors make Making Clothes, Sewing, Needles and Thread, Mattresses and Upholstery and shoemaking (Footwear) fast and accurate; sheep shears make Wool a crop rather than a moult; snips make every can and bucket in Tins, Cans, Drums and Tanks; pruning shears keep Fruit Trees and Orchards bearing. The same skills — matched pairs, pivots, springs and fine heat treatment — lead to surgical scissors (Medical Instruments), Razors, Nail Clippers and Grooming Tools, and the precise work of Locks and Keys and Scientific Instrument Making.

How it was first done

Spring shears appear in Europe in the Iron Age, by about the 5th–3rd centuries BC, and spread across the Roman world; the same design is still sold for sheep shearing. Pivoted scissors were used by the Romans by the 1st century AD, but remained less common than spring shears in Europe until the later Middle Ages. In the 18th century Sheffield in England became the great centre of scissor and knife making; there Robert Hinchliffe is said to have been first to make scissors from crucible ("cast") steel, in 1761. Pruning shears are generally credited to the Frenchman Antoine-François Bertrand de Molleville around 1815.

Folding knives without springs were made in the Iron Age and by the Romans. Knives with a back spring spread in the 17th and 18th centuries; the penknife, small enough to trim quill pens (Pens, Nibs and Writing Instruments), became an everyday tool. The Swiss army knife, with several blades on back springs, dates from the 1890s. Butcher's steels were standard in the 19th century.

Source: content/entries/metals/scissors-and-shears.md