◆ Rebuild

Part 3 · Metals

Metal Pipes and Tubes

How to make metal tube — rolled from strip and soldered, brazed or forge-welded along the seam, drawn thinner and truer through dies over a plug, or pierced seamless from a solid billet — and how to bend it, thread it and join it into pipework for water, gas and steam, boilers and bicycle frames.

Difficulty
●●●●●
Time
An afternoon to braze a short brass tube; a day to forge-weld a metre of iron pipe by hand; months to set up a tube mill
Steps from zero
28 prerequisites →

You need first

Sheet Metal and RollingWelding

This unlocks

Burners, Stands and Laboratory EquipmentSyringes and Hypodermic NeedlesPressure and Vacuum Gauges

Objects made here

pipetubedraw benchboiler
The full path from nothing — 28 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. The Kiln
  11. Hides and Leather
  12. Bricks
  13. Lime
  14. The Wheel and Axle
  15. Firebrick and Refractories
  16. Bellows
  17. Gears
  18. Iron (the Bloomery)
  19. Copper Smelting
  20. The Waterwheel
  21. Blacksmithing
  22. Magnets
  23. Sheet Metal and Rolling
  24. Copper Wire
  25. The Generator
  26. The Electric Arc Furnace
  27. Calcium Carbide and Acetylene
  28. Welding
  29. Metal Pipes and Tubes

Do them roughly in this order. See it on the tech tree →

Why it matters

Tube carries things and holds things. Pipes bring water into houses and towns (Pipes, Plumbing and Aqueducts), carry coal gas and air (Bellows to Air Compressors), and take steam from the boiler to the engine (Boilers and Pressure Vessels, The Steam Engine). Hundreds of small tubes inside a boiler pass the fire's heat to the water. Condensers, stills, refrigerators and heat exchangers are mostly tube (Distillation, Ice and Refrigeration, Heat Exchangers). Hydraulic presses and brakes need tube that holds hundreds of bar (Hydraulic Presses and Rams).

Tube is also the strongest shape for its weight. A round tube resists bending and twisting far better than a solid bar of the same weight, because its metal sits out at the edge where the stress is greatest. That is why bicycle frames, scaffolding, masts, telescope bodies and aircraft frames are made of tube (The Bicycle, Scaffolding and Ladders, The Telescope, Gliders and Aeroplanes).

Wood, clay and lead pipes come first and still have their uses (Pipes, Plumbing and Aqueducts, Tiles and Clay Pipes, Lead). Iron, steel, copper and brass tube is what pressure and machinery demand.

How it works

Pressure and wall thickness. Pressure inside a pipe tries to split it lengthways. The force on the wall grows with the pressure and the diameter, so:

wall thickness = pressure × diameter ÷ (2 × allowable stress)

— the same rule as for a boiler (Sheet Metal and Rolling, Boilers and Pressure Vessels). Small pipes therefore stand huge pressures with thin walls. A 60 mm wrought-iron pipe with a 3.6 mm wall could, on paper, hold about 60 bar (using an allowable stress of 50 MPa). But threads cut into the wall, rust eats it and a poor seam weakens it, so ordinary threaded iron pipe is used at 10–20 bar at most.

The seam is the weak point. Most tube starts as a flat strip (called skelp) bent round until its edges meet. Those edges must then be joined: by solder or brass (for copper and brass tube), or by welding them into one piece of iron. A seam with slag in it, or edges that only stuck instead of fusing, splits under pressure. Seamless tube, pierced from a solid bar, avoids the problem but needs heavy machinery.

Drawing makes tube better. Pulling a tube through a hard die — over a plug inside it — squeezes the wall thinner, makes it smooth and exact in size, and hardens the metal (Iron and Brass Wire). As with wire, the metal must be annealed (softened by heating) every few passes or it cracks.

What you need

Item Notes
Strip (skelp) Iron or mild steel for welded pipe; copper or brass for brazed tube. Width = π × outside diameter (+ the overlap for a lap seam). Thickness 2–4 mm for pipe, 0.7–1.5 mm for light tube (Sheet Metal and Rolling)
Forge with a long fire A trough fire about 20 cm long, so a section of tube heats evenly (Blacksmithing)
Swage block or grooved bottom tools Half-round grooves of the finished sizes
Mandrels Round steel bars, a little smaller than the bore, 1–2 m long
Welding bell A short, thick iron or steel cone with a polished bore of the finished size (for butt-welded pipe)
Draw bench Chain or rope pulled by a winch, gearing or water power (Iron and Brass Wire)
Dies and plugs Hardened steel: ring dies of each size and bullet-shaped plugs on long rods
Flux Borax for brazing, clean sand or borax for forge welds (Soldering and Brazing)
Pipe threading Die stock with pipe dies, pipe vice, pipe wrench or chain tongs (Screws, Nuts and Bolts)
Jointing Hemp fibre, and a paste of linseed oil with chalk or graphite (Flax, Hemp and Linen)

Method 1: Brazed and soldered tube

The easiest tube, for copper, brass and tinplate: lamp bodies, instrument tubes, telescopes, stills, small water pipes, early bicycle frames.

  1. Cut the strip to width: for a 20 mm tube, π × 20 = 63 mm, plus 4–6 mm if you will overlap the edges.
  2. Form it. Bend the strip into a U by hammering it into a half-round groove in a swage block or a hardwood block with a mallet; then close it round a mandrel with a mallet until the edges meet or overlap. Anneal copper and brass when they stiffen: heat to a dull red and let cool (quench copper in water).
  3. Bind the tube every 5–8 cm with soft iron wire so the seam stays closed.
  4. Flux and join. For soft solder (low pressure, low heat), clean the seam bright, paint on flux, and run solder along it with a big soldering iron (Soldering and Brazing). For brazing (strong, and good to about 200 °C), sprinkle borax paste along the seam, lay a thin strip of brass or spelter along it, and heat a short length at a time to bright orange (about 900 °C) until the brass runs into the joint and shows as a thin line along both sides.
  5. Clean off the flux glass with hot water and a wire brush. Draw the tube through one or two dies over a plug (Method 3) to make it round, smooth and exact.

A brazed seam drawn afterwards is good enough for bicycle frames, light steam pipes and condenser tubes.

Method 2: Forge-welded iron pipe

Butt weld: pulled through a bell flat skelp curling in the bell edges pressed and welded White-hot strip from a long furnace, edges bevelled Welding bell funnel-shaped die Tongs and chain to the draw bench Lap weld: rolled over a ball Groovedroll Groovedroll Scarfed edges overlapand are pressed into one piece Tube at welding heat Ball insideheld on a long rod where the rolls pinch By hand: scarf both edges, bend round a mandrel, weld 10–15 cm at a time at a bright yellow-white heat (about 1,300 °C), hammering the overlap down over a mandrel and rounding it in a swage.
Fig. 1 Two ways to weld a seam. In a butt weld the strip is pulled white-hot through a bell, which presses the edges together. In a lap weld the scarfed edges overlap and are hammered or rolled together over a mandrel.

This is how most iron pipe was made for a century, first by hand, then by machine.

By hand (lap weld)

  1. Prepare the skelp. Cut wrought iron or mild steel strip 2.5–4 mm thick, π × outside diameter plus about 3 times the thickness wide. Scarf (bevel) both long edges at the forge so they taper over about 2–3 times the thickness, on opposite faces, so they overlap smoothly.
  2. Bend the skelp red-hot into a U in a swage, then close it round a mandrel so the scarfs overlap.
  3. Weld a section. Pull the mandrel out (it would weld in!). Heat 10–15 cm of the seam in a long, clean charcoal or coke fire to welding heat — a bright yellow-white, almost too bright to look at, with tiny sparks starting to spit from the surface (about 1,300 °C) — sprinkling sand or borax on the seam as it reaches orange to dissolve the scale (Blacksmithing).
  4. Close it. Quickly slip the hot section over a mandrel held in a vice or a hole in the anvil, seam up, and hammer the overlap down with quick, firm blows, then round it in a swage. Work from the middle of the heat outward to squeeze out slag.
  5. Move along. Reheat the next 10–15 cm, overlapping the last weld by a few centimetres, and repeat. A smith and striker can weld a metre of 50 mm pipe in an afternoon.
  6. Size it by passing it hot through a swage or bell of the finished size.

By machine

  • Butt welding (for small pipe, up to about 75 mm). The flat skelp, its edges slightly bevelled, is heated white-hot along its whole length in a long furnace. One end is gripped with tongs and pulled through a bell — a funnel-shaped die — by a chain on a draw bench. The bell curls the strip round and presses the edges together so hard that they weld. A second pass through a smaller bell, or between grooved rolls, finishes the size.
  • Lap welding (for bigger pipe). The skelp is first bent round with overlapping scarfed edges, then reheated to welding heat and pushed between a pair of grooved rolls with a round, egg-shaped ball held on a long rod inside the tube at the point where the rolls pinch. The rolls press the overlap against the ball and weld it.

By gas or electric welding

With oxy-acetylene or an electric arc (Welding), you can roll strip into tube cold and weld the butted edges in one long run — the method behind most modern pipe. Practise on short lengths, and test every pipe (below).

Method 3: Drawn tube

Hardened ring diefixed to the bench Thick, rough shell Thinner, smooth, exact Plugsets the bore; heldon a rod Rod anchoredat the back of the bench Pointed endgripped and pulledby the bench chain
Fig. 2 Tube drawing on a bench. The tube's pointed end is gripped and pulled through a hard ring die, while a plug held on a rod inside sets the bore. The wall comes out thinner, smoother and exact.

Drawing turns rough, thick tube — brazed, welded, cast or pierced — into smooth, thin, exact tube. It is how copper and brass tube, boiler tubes, bicycle tubes and instrument tubes are finished.

  1. Start with a shell. Any of: a brazed or welded tube; a thick tube cast in brass or copper round a dry sand or clay core (Metal Casting); or a cup pressed from a disc in several stages and then its bottom cut off.
  2. Point the end. Hammer one end down for 10–15 cm so it passes through the die and can be gripped.
  3. Lubricate inside and out: tallow with soap, or soap solution for brass; the old lime coat for iron (Iron and Brass Wire).
  4. Draw. Choose one of three ways:
    • Sinking — no plug inside. The tube's outside shrinks and its wall stays about the same. Good for small changes in size.
    • Plug drawing — a hardened plug on a long rod, anchored at the back of the bench, sits inside the tube level with the die. The tube is squeezed between die and plug; the wall gets thinner and the bore exact. The usual method.
    • Mandrel drawing — a long hard bar is pushed inside the tube and drawn through with it, then the tube is loosened by rolling it and the bar pulled out. Gives very thin walls and long lengths.
  5. Reduce gradually. Each pass should take off no more than about a quarter of the tube's cross-sectional metal. Anneal after every two or three passes: copper and brass at a dull red (about 600 °C), steel at a dull cherry red (about 700 °C) in a closed pot or under charcoal. Pickle off the scale in weak acid before the next draw (Acids, Bases and Testing).
  6. Straighten by rolling the tube between a board and a flat bench, or between two slightly skewed rollers.

Butted tube for bicycles is drawn over a mandrel shaped with thicker ends: the walls are thick where tubes are brazed into lugs and the stress is highest, and thin in the middle to save weight (The Bicycle).

Method 4: Seamless tube (in outline)

Seamless tube is made by forcing a hole through a hot solid billet. Two classic ways:

  • Cross-roll piercing (the Mannesmann process, 1885–86). A round billet, white-hot, is fed between two barrel-shaped rolls set at a slight angle to each other. They spin the billet and drag it forward; the squeezing pulls its centre apart, and a pointed piercing plug on a rod opens it into a thick shell. The shell is then rolled and drawn to size.
  • Pushing (the Ehrhardt process, 1891). A square billet in a round die is pierced by a hydraulic punch into a closed-ended cup, which is then pushed by a ram through a row of dies on a long bench.

Both need heavy powered mills (Hydraulic Presses and Rams, The Steam Engine) and very hard tool steel (Alloy and Stainless Steels). For soft metals there is a much easier seamless method: extrusion. Lead is squeezed out through a ring-shaped gap between a die and a central rod by a screw or hydraulic press, giving lead pipe of any length (Lead).

Bending pipe

  • Bend small soft copper tube cold round a wooden or iron former, by hand.
  • For anything bigger or harder, fill the tube first so it does not flatten or kink: plug one end with a tight wooden bung, fill it with completely dry fine sand, tapping it all the time so the sand packs solid, and plug the other end. (For thin brass, fill with melted rosin or lead instead and melt it out afterwards.)
  • Heat the bend area evenly to a dull red (iron) or anneal it (copper and brass), and pull it slowly round a former, never sharper than 3–4 times the pipe's diameter for the inside radius.
  • A coiled steel spring slipped inside or over a small soft tube also stops it kinking.

Threading and joining

Socketcast malleable iron or brass, threaded inside Tapered threadnarrows 1 in 16 ondiameter (exaggerated) Pipe wallthread cut with a die stock Hemp and jointing pastewound into the threads; the joint tightensand seals as the taper wedges home
Fig. 3 Joining threaded pipe. Both pipe ends carry a tapered thread; they screw into a socket and tighten as they go in. Hemp and jointing paste in the threads seal the joint.

Pipe threads are tapered: the thread narrows toward the pipe's end by 1 in 16 on the diameter (about 1 mm narrower for every 16 mm along). As the pipe screws into a fitting, it wedges tighter and seals. The British standard (Whitworth) form has a 55° thread angle.

Nominal size Outside diameter Threads per inch (25.4 mm)
½ inch 21.3 mm 14
¾ inch 26.9 mm 14
1 inch 33.7 mm 11
1½ inch 48.3 mm 11
2 inch 60.3 mm 11

The nominal size was once about the bore, not the outside. Whatever sizes you choose, standardise them in your community so every pipe fits every fitting (Precision and Interchangeable Parts, Measurement from Scratch).

  1. Cut the pipe square with a hacksaw or a wheel cutter, and file off the burr inside.
  2. Clamp it in a pipe vice close to the end.
  3. Thread it with a die stock — a split, adjustable pipe die in a frame with two long handles. Oil generously; turn forward half a turn, back a quarter turn to break the chip. Stop when the pipe's end is level with the far face of the die. Make dies and taps as in Screws, Nuts and Bolts.
  4. Seal. Brush jointing paste (linseed oil worked stiff with chalk or graphite) on the thread, wind a few strands of hemp into the thread grooves in the direction of the thread, add more paste, and screw on the fitting by hand, then tighten with a wrench two or three turns more.
  5. Fittings — sockets (straight couplers), elbows, tees and caps — are cast in malleable iron or brass and tapped (Metal Casting, The Blast Furnace and Cast Iron). A union (two halves that join with a big nut) lets you take a pipe run apart without unscrewing every joint.

Other joints.

  • Flanges for big pipes and steam: a flat ring on each pipe end, screwed or welded on, bolted together with a gasket between them — oiled card, rubber (Rubber), copper or lead ring (Packing, Gaskets and Seals).
  • Soldered (sweated) sockets for copper water pipe: the pipe end pushed into a close-fitting socket, both tinned, and heated until solder runs in.
  • Flared and compression joints for small copper tube on instruments and fuel lines: the tube end spread into a cone and squeezed by a nut, or a soft brass ring crushed onto it.
  • Boiler tubes pass through holes in the tube plates and are expanded — a tapered tool with rollers is driven into the tube end and turned, swelling the tube until it grips the hole tight — then the end is turned over (beaded) (Boilers and Pressure Vessels).

How to tell it worked

  • Look and ring. Tap a pipe with a hammer: it should ring clear. A dull spot can mean a bad weld.
  • Flattening test. Cut a ring 5 cm long from each batch and squash it in a vice, seam at the side, until the walls nearly touch. A good welded or brazed seam does not open; a bad one splits along the seam.
  • Bend test. A short length filled with sand should bend 90° cold round a former 6 times its diameter without cracking.
  • Water test. Fill the pipe or finished pipework with water (not air), drive out every bubble, and pump it to 1.5–2 times the working pressure with a hand pump and a gauge (Pressure and Vacuum Gauges). Hold for 10 minutes. Any weep, drip or falling gauge means a leak. See Boilers and Pressure Vessels for the method.

Note Troubleshooting. Forge weld opens when flattened, showing a dark, scaly line → edges were not at welding heat, or scale was trapped. Clean flux, hotter fire, faster hammering, and scarf the edges longer. Pipe burned and crumbly in patches → overheated: white sparks pouring off means the iron itself is burning. Pull it from the fire sooner. Brazed seam has gaps → seam not clean, or not hot enough along its whole width. Clean bright, more borax, heat both sides evenly. Tube splits during drawing → too big a reduction per pass, or not annealed. Smaller steps, anneal more often. Tube breaks off at the point → pointed too thin, or the die is rough. Make a longer, thicker point; polish the die. Threaded joint weeps → thread cut too short or too deep, or no hemp. Recut, and use hemp and paste. Pipe kinks on bending → sand not packed hard, or bend too tight. Repack, and use a larger former.

Dangers

Danger Wet sand in a heated pipe explodes. Any water in the sand turns to steam, which can blow a plug out like a bullet or burst the pipe. Dry the sand thoroughly over a fire first, and never stand in line with a plugged pipe's ends while heating it.

Danger Never pressure-test with air. A pipe full of compressed air that bursts releases its stored energy at once and throws fragments; a pipe full of water that bursts just leaks, because water barely compresses. Always test with water, with all the air let out. See Bellows to Air Compressors and Boilers and Pressure Vessels.

  • Forge welding sprays white-hot scale. Wear leather and protect your eyes; keep onlookers back 3 m. See Blacksmithing.
  • Zinc fumes. Heating, welding or brazing galvanised pipe gives off white zinc oxide fumes that cause metal fume fever — shivering and fever like flu a few hours later. Work outdoors, upwind, or file off the zinc first (Zinc and Brass).
  • Lead pipe and lead-based jointing paste poison drinking water slowly. Prefer copper, iron or clay pipe for drinking water and lead-free paste. See Lead.
  • Draw benches store great force in the chain. If a tube or grip breaks, the chain and tongs whip back. Stand to the side.

What this unlocks

Pressure water mains and house plumbing (Pipes, Plumbing and Aqueducts, Firefighting); steam pipes and fire-tube and water-tube Boilers and Pressure Vessels; condensers and heat exchangers for Distillation, Ice and Refrigeration and the The Steam Turbine; hydraulic lines (Hydraulic Presses and Rams); gas lighting and fuel lines (Petroleum and Refining, The Internal Combustion Engine); bicycle and aircraft frames (The Bicycle, Gliders and Aeroplanes); tube scaffolding (Scaffolding and Ladders); telescope and instrument bodies (The Telescope, The Barometer).

How it was first done

The Romans made water pipes (fistulae) by bending cast lead sheet round a rod and soldering or folding the seam; wooden and clay pipes served most towns for centuries after. Cast iron water mains came in the 1600s — the great pipes of the Marly machine that fed the fountains of Versailles were laid in the 1680s. When gas lighting began in Britain around 1800, the first gas pipes were often old musket barrels screwed end to end. In 1825 Cornelius Whitehouse of Wednesbury, England, patented the butt-welding of pipe by drawing hot skelp through a bell, and the lap-welding of larger tube between rolls followed in the 1830s and 1840s, making boiler tubes and gas pipe cheap. In Germany in 1885–86 the brothers Reinhard and Max Mannesmann invented cross-roll piercing of seamless tube, and Heinrich Ehrhardt introduced his push-bench method in 1891. Cold-drawn seamless steel tube made the lightweight bicycle of the 1890s possible; the British firm of Alfred Reynolds patented butted tube in 1897.

Source: content/entries/metals/metal-tubes.md