◆ Rebuild

Part 3 · Metals

Enamel on Metal

Vitreous enamel is a thin coat of glass fused onto iron, steel or copper. It turns rusting sheet iron into cooking pots, basins, bathtubs and signs that last for decades and clean like a plate, and turns copper and gold into jewellery. This chapter covers making a lead-free enamel glass, preparing the metal, the ground coat that makes glass stick to iron, firing in a muffle, and the common faults.

Difficulty
●●●●●
Time
A week to make and test a frit; an hour to coat and fire a piece; months of trials before cookware is reliable
Steps from zero
22 prerequisites →

You need first

GlazesSheet Metal and Rolling

This unlocks

—
The full path from nothing — 22 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Pottery
  9. The Kiln
  10. Charcoal
  11. Hides and Leather
  12. Lime
  13. Lye and Potash
  14. The Wheel and Axle
  15. Glass
  16. Bellows
  17. Gears
  18. Glazes
  19. Iron (the Bloomery)
  20. The Waterwheel
  21. Blacksmithing
  22. Sheet Metal and Rolling
  23. Enamel on Metal

Do them roughly in this order. See it on the tech tree →

Why it matters

Iron is strong and cheap but rusts, and it taints acid food. Copper is beautiful but turns green and poisons vinegar. Clay pots are clean but break. Enamel gives you the best of both: the strength of metal with the clean, hard, waterproof, rust-proof surface of glass.

With it you can make:

  • Cookware and kitchenware — pots, kettles, mugs, plates, basins and buckets that do not rust, do not taint food and wash clean (Kitchen and Cooking).
  • Sanitary ware — washbasins, baths, bedpans and hospital trays that can be scrubbed and boiled (Sanitation and Germs, Sterilising Instruments and Dressings).
  • Signs — street names, notices and milestones that keep their colour outdoors for fifty years.
  • Instrument dials and clock faces (The Mechanical Clock), labels for laboratory and pharmacy jars.
  • Jewellery and decoration on copper, silver and gold — the coloured cells of cloisonné.
  • Later, linings for chemical tanks and water heaters that resist acid and rust.

How it works

Enamel is a glaze for metal. Like the glazes of Glazes, it is glass — silica made to melt by a flux, and stiffened a little with alumina — ground to powder, laid on, and melted in a kiln. But metal is harder to glaze than clay, for three reasons:

  1. It must melt below the metal's danger point. Sheet iron sags and scales badly above about 900 °C; copper melts at 1,085 °C and oxidises fast long before. So enamel must flow at 750–850 °C — much softer glass than window or bottle glass. The flux that does this best without lead is borax, with soda.
  2. It must shrink like the metal. Metals shrink a lot as they cool — copper even more than iron — and ordinary glass much less. If the glass shrinks far less than the metal, the cooling metal crushes it and it flakes off ("spalls"). Soft, alkali-rich, borax glass shrinks more, close to the metal. Ideally the glass shrinks a little less than the metal, so it ends up gently squeezed, which glass resists very well.
  3. It must stick. Glass does not stick to clean steel by itself; it rolls up into beads. Two things make it grip:
    • A thin layer of iron oxide on the metal surface dissolves into the glass during firing and binds the two.
    • A ground coat containing tiny amounts of cobalt and nickel oxides. These react at the steel surface and roughen it microscopically, so the glass anchors itself. This is why the first coat on enamelled iron is nearly always dark blue-grey or black. On copper and gold, the metal's own oxide does the job, and no ground coat is needed.

A finished piece of enamelled steel is a sandwich: steel, a grey-blue ground coat 0.1–0.2 mm thick, and one or two white or coloured cover coats on top, 0.2–0.5 mm in all. Thin is strong: thick enamel chips.

Enamelled sheet steel, magnified total enamel 0.2–0.5 mm a side; thin is strong Cover coatwhite or coloured, 0.1–0.3 mm Ground coatblue-black; cobalt and nickelroughen the steel and grip it Steel or iron sheetlow carbon, 0.6–1.5 mm, clean and pickled Ground coaton the back too Back coatbalances the stress, stops curling Sharp edgecoat thin at the corner: chips Rounded edgeeven coat: holds Round every edge to at least 2–3 mm, or roll it over a wire, before enamelling.
Fig. 1 Enamel on steel in cross-section. The ground coat grips the steel; the cover coat gives the colour. Thin sheet is enamelled on both sides so the stresses balance.

What you need

Item Notes
Frit ingredients Quartz or clean sand, feldspar, borax, soda ash or natron, fluorspar; colourants (below)
Crucible Fireclay, 2–5 litres, for melting frit at 1,100–1,250 °C (Firebrick and Refractories)
Furnace reaching 1,250 °C For frit melting; a good The Kiln or a forge with a strong blast (Bellows)
Muffle kiln reaching 850–900 °C For firing the ware: a clay box heated from outside, so no flame or ash touches the work
Ball mill or mortar For grinding frit fine: a stoneware jar of hard pebbles rolled for a day, or a stone mortar (Stoneware and Porcelain)
Sieves Silk or fine brass gauze, about 60–80 threads per cm for wet enamel
Metal Low-carbon sheet iron or mild steel 0.6–1.5 mm thick (Sheet Metal and Rolling); cast iron; copper sheet 0.6–1 mm
Pickle Weak sulfuric acid (Sulfuric Acid) or vinegar (Vinegar and Pickling); soda water for rinsing
Tools Iron fork or wire rack to carry work into the kiln, long tongs, a spatula, brushes, a dusting sieve

Where to find it

  • Quartz, sand and feldspar: see Glass and Stoneware and Porcelain. For enamel, use clean white quartz or white sand with no rust stain: iron spoils white enamels.
  • Borax (Borax and Boric Acid): white crusts on dry salt lakes in deserts (Tibet, Turkey, the American West, the Andes). Tastes sweetish-alkaline, dissolves in hot water, and a bit heated on charcoal swells up like popcorn and then melts to a clear glass bead. Without borax, a soda-potash glass with extra feldspar will work on iron, but it melts hotter and fits less well.
  • Soda: Soda Ash and Baking Soda from plant ashes or natron lakes.
  • Fluorspar (fluorite): glassy cubes, purple, green, yellow or colourless, in veins with lead ores; softer than quartz. A few percent makes the enamel flow and turns it milky.
  • Colourants and opacifiers: tin oxide from roasting tin (Tin and Pewter) gives white; cobalt ore gives blue (and is part of every iron ground coat); nickel ore (green garnierite) or nickel and cobalt compounds made as in Nickel and Cobalt; manganese ore (black, sooty) gives brown and purple; iron oxide gives brown and black; copper gives green. See Glazes.

Step 1: Make the frit

A frit is enamel glass made once in a crucible, quenched in water and ground. Melting it first locks the soluble borax and soda into glass and gets rid of gas, so the coat does not bubble.

Ground coat for iron and steel (by weight, approximate — test and adjust):

Ingredient Parts
Borax 30
Feldspar 28
Quartz 20
Soda ash 8
Fluorspar 5
Manganese oxide 1.5
Nickel oxide 1–1.5
Cobalt oxide 0.5

White cover coat (by weight):

Ingredient Parts
Borax 26
Quartz 30
Feldspar 25
Soda ash 10
Fluorspar 6
Saltpetre (helps keep colours clean, Saltpeter) 3

Soft enamel for copper and silver jewellery: borax 30, quartz 35, soda ash 20, potash 15, plus colourants. It flows at about 750–800 °C.

  1. Weigh and mix the ingredients dry, ground together fine enough to pass a kitchen sieve.
  2. Melt in a fireclay crucible at 1,100–1,250 °C — yellow to yellow-white heat — for 1–2 hours, until a thread pulled out on an iron rod is clear and free of bubbles and lumps. Melt outdoors: fluorspar and borax give off sharp fumes.
  3. Quench. Pour the melt in a thin stream into a big tub of cold water. It shatters into glassy grains, which are far easier to grind than a solid lump.
  4. Dry the grains.

Step 2: Grind and make the slip

For wet application (iron and steel ware):

  1. Grind, by weight: 100 parts frit, 5–7 parts plastic white clay (it keeps the powder suspended), 40–50 parts water, and for the white cover coat 6–10 parts tin oxide. Grind in a pebble mill for 12–24 hours, or by hand in a stone mortar, until nearly all passes your finest sieve.
  2. Adjust with water to a slip like thin cream. Too thin runs and leaves bare patches; too thick piles up and chips. A finger dipped in it should be just hidden.
  3. Add a pinch of borax or salt (about 0.2 parts) if the slip settles too fast or runs off the work: it "sets up" the clay.

For dry application (jewellery and cast iron): grind the frit dry in a mortar, sieve it to the fineness of flour, and wash it several times in water, pouring off the cloudy fines, which make enamel dull. Dry it.

Step 3: Prepare the metal

The metal must be clean, free of grease, and free of scale. Most failures start here.

Sheet iron and steel:

  1. Shape first. Bend, spin or press the pot or plate to its final shape (Sheet Metal and Rolling). Round every edge and corner — at least 2–3 mm radius — or roll it over a wire (Iron and Brass Wire). Enamel always chips first on sharp edges. Rivets and seams must be smooth and tight; welded or lock-seamed joints, not soldered — solder melts in the kiln.
  2. Use low-carbon iron. Carbon in the metal turns to gas in the kiln and bubbles up through the enamel. Wrought iron and soft mild steel are best; never enamel tool steel.
  3. Burn off grease: heat the piece to a dull red (about 600 °C) for a few minutes and let it cool.
  4. Pickle: 15–30 minutes in warm weak sulfuric acid (about 1 part acid to 15–20 parts water), or a day in strong vinegar, until bright and grey all over. Scrub with sand.
  5. Rinse in clean water, then in water with a handful of soda ash per bucket to kill the last acid, and dry at once in a warm place. Enamel within a few hours, before rust appears.

Copper: anneal, pickle in vinegar with salt, scrub bright with pumice or fine sand, and do not touch the clean surface with fingers.

Cast iron: sand off the casting skin by scouring with sharp sand and water, or by tumbling, and enamel the next day.

Step 4: Apply and fire

Chimneygives the draught Mufflefireclay box, walls 3–4 cm;inside 800–870 °C, cherry to orange Work on an iron rackno flame or ash touches it Door with peepholewatch for the gloss Flames pass roundunder, beside andover the box Fire on a gratewood or charcoal Brick orclay body air in Seen from the side. A test chip that glazes in 3–4 minutes shows the kiln is ready.
Fig. 2 The muffle kiln. The fire heats a clay box; the work sits inside it on an iron rack, away from flames and ash. A small peephole shows when the enamel has turned glossy.

The muffle. Build a clay box about 40 × 30 × 25 cm inside, with walls 3–4 cm thick of fireclay and grog (Firebrick and Refractories), open at the front with a clay door. Build a firebox round it so flames pass under, round the sides and over the top, then up a chimney. Preheat it until the inside glows bright cherry to orange — about 800–870 °C. A test chip of your enamel on a scrap of metal tells you better than any colour: when it fires glossy in 3–4 minutes, the kiln is right.

Iron and steel ware:

  1. Dip or pour the ground coat slip over the piece, inside and out, and drain it, turning it so the coat is even. Wipe the rim clean if it is to be beaded later.
  2. Dry it completely — a few hours in a warm place, or near the kiln. The dry coat looks like chalk and must not be touched.
  3. Fire: slide the piece into the muffle on an iron fork or wire rack. In 2–5 minutes (longer for heavy pieces) the coat goes from grey powder to a rough "sugary" surface, then to a smooth gloss. Take it out as soon as the whole surface is glossy.
  4. Cool slowly in still air, out of draughts, on a rack.
  5. Cover coat: apply the white or coloured slip, dry, and fire again, a little cooler (780–820 °C). A second cover coat gives better whiteness.

Signs: cover-coat a flat plate white, fire, then lay a paper or thin sheet-metal stencil over it, sift or brush on a second colour, lift the stencil, and fire again. One firing per colour.

Cast iron pots (the dry method): heat the cleaned pot to bright red in the muffle, pull it out, and quickly dust the dry enamel powder through a sieve onto the hot surface, where it sticks and starts to melt. Return it to the kiln for a few minutes to flow. Repeat for a second coat.

Copper jewellery:

  1. Brush a little thin gum water (gum arabic or quince seed water) on the clean copper, and sift dry enamel onto it, about 0.3 mm thick.
  2. Counter-enamel: give the back a coat of any scrap enamel. Thin copper with enamel on one side only curls and cracks as it cools.
  3. Dry, and fire at 750–820 °C for 1–3 minutes, until glossy.
  4. Cloisonné: bend flat strips of fine copper, silver or gold wire, about 1 mm tall, into the outline of the design, set them on edge on a fired base coat, and fire them in place. Fill each little cell with wet enamel of one colour, fire, fill again — enamel shrinks — and fire until the cells are level. Stone the surface flat with wet sandstone (Abrasives and Grinding Stones) and refire briefly to restore the gloss.
  5. Champlevé: instead of wire, cut or etch hollows into thick metal and fill them with enamel.

How to tell it worked

  • Gloss and colour. The surface is smooth and glassy all over, with no bare spots, pinholes or bubbles. White is white, not grey or speckled.
  • Ring. Tap an enamelled pot with a fingernail: it rings clearly. A dull note can mean a hidden crack.
  • The bend and tap test (on a test strip only). Bend a narrow enamelled strip a little, or tap its back with a hammer: well-bonded enamel cracks, but the bits cling to the metal, which still shows blue-grey patches of ground coat where they broke. If the enamel pops off clean and leaves bright bare steel, it never stuck.
  • The boil test. Boil water with a little vinegar in a new pot for an hour. The enamel should come out unchanged.
  • The thermal test. Heat an empty pot over a gentle fire till a drop of water dances on it, and plunge it into cold water. Good enamel survives.

Note Troubleshooting. Enamel crawls into beads and leaves bare metal → grease or dirt on the metal. Burn off and pickle better. Bubbles and pinholes → coat not fully dry; carbon in the steel; or rust on the metal. Dry longer, use lower-carbon iron, enamel soon after pickling. Small half-moon flakes pop off hours or days after firing ("fish-scaling") → hydrogen trapped in the steel, usually from long acid pickling or wet coats. Pickle shorter, dry thoroughly, add a little more clay to the ground coat, and heat the bare piece to dull red before coating. Enamel chips at edges → edges too sharp, or coat too thick. Round the edges; apply thinner coats. Fine crack network (crazing) → the enamel shrinks more than the metal. Add quartz, reduce soda. Whole patches flake off → the enamel shrinks much less than the metal, or the ground coat failed. Add soda or borax; check the cobalt and nickel in the ground coat. Black or burnt edges → fired too hot or too long. Shorten the firing. Rough, sugary surface → underfired. Fire a little longer or hotter. Grey, dirty white → iron in the raw materials, or fire gases in the muffle. Use purer quartz and seal the muffle.

Dangers

Danger Never use lead in enamel for anything that touches food or drink, and do not trust old coloured enamels of unknown make for cooking: many contained lead, cadmium or antimony. Acid foods leach them out (see Glazes on lead). The recipes in this chapter are lead-free.

Danger Silica dust scars the lungs. Grinding quartz, feldspar and frit dry makes a fine dust that causes silicosis — slow, permanent, deadly lung damage. Grind wet whenever you can, sweep only when damp, and cover your nose and mouth with a damp cloth during any dry work.

  • Hot ware looks the same hot as cold. Mark the cooling rack and use tongs.
  • Frit melting gives off fumes from fluorspar (fluorine compounds that attack the lungs and eyes) and borax; melt outdoors, upwind, and keep out of the smoke. Quenching molten glass in water throws steam and hot fragments — pour in a thin stream, and stand back.
  • Acid pickle: add acid to water, never water to acid; wear eye protection (Sulfuric Acid).
  • Cobalt, nickel and manganese powders are poisonous; wash hands, keep them away from food. Cobalt ores often carry Arsenic: roast them only as that chapter describes.
  • Chipped cookware: a chip exposes iron, which rusts but is harmless. Discard pots whose enamel is flaking into food.

What this unlocks

Rust-proof Kitchen and Cooking, basins and buckets; washable hospital and laboratory ware (Sterilising Instruments and Dressings, Laboratory Glassware); signs and milestones (Roads and Bridges); dials for clocks and instruments (Measuring Electricity); jewellery and decoration. Glass-lined steel tanks lead on to chemical plant for Sulfuric Acid and Chlorine and Bleach and to hot-water cylinders (Pipes, Plumbing and Aqueducts). The same glass-on-metal joint is how wires are sealed through glass in a The Light Bulb and a The Vacuum Tube.

How it was first done

The oldest known enamel is on six gold rings from a 13th-century BC tomb at Kouklia in Cyprus. Celtic smiths of the last centuries BC fused red glass onto bronze shields and horse harness. Byzantine goldsmiths made exquisite cloisonné in the 500s–1100s AD, and from the 1100s the workshops of Limoges in France turned out champlevé enamel on copper for church furniture across Europe; Limoges later became famous for painted enamels. Chinese cloisonné flourished under the Ming dynasty from the 1400s.

Enamelling iron for everyday use came in the 1800s. Enamelled cast-iron pots were made in Germany from the early 1800s, and by mid-century German and Austrian works were enamelling pressed sheet iron. In the 1870s the Niedringhaus brothers of St. Louis made mottled grey "graniteware", which spread enamelled cooking pots across America. The discovery that small amounts of cobalt and nickel in the ground coat made enamel grip steel reliably was what made cheap enamelled steel possible; enamelled street signs, advertising plates and bathtubs followed from the 1890s.

Source: content/entries/metals/vitreous-enamel.md