Part 14 · Electronics and Computing
Quartz Crystals and Frequency Control
A thin plate of quartz rings like a bell when you give it an electric push, at a frequency fixed by its thickness and almost untouched by heat. Ground to size from natural rock crystal with emery and a glass plate, and set in a one-tube oscillator, it holds a radio transmitter on its channel to a hundredth of a per cent, and can run a clock better than any pendulum.
- Difficulty
- ●●●●●
- Time
- A week to find, saw and grind a first crystal; a season to make a set of channel crystals and a quartz clock
- Steps from zero
- 28 prerequisites →
The full path from nothing — 28 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- The Kiln
- Pottery
- Charcoal
- Abrasives and Grinding Stones
- Hides and Leather
- Lime
- Mercury
- Lye and Potash
- Fermentation
- The Wheel and Axle
- Glass
- Bellows
- The Lathe
- Copper Smelting
- Laboratory Glassware
- Pumps
- The Battery
- The Vacuum Pump
- The Light Bulb
- The Vacuum Tube
- Amplifiers and Oscillators
- Quartz Crystals and Frequency Control
Do them roughly in this order. See it on the tech tree →
Why it matters
An oscillator built from a coil and a capacitor (Amplifiers and Oscillators) drifts. Warm the coil and it stretches; change the battery voltage, move your hand near it, or let the damp in, and the frequency wanders by a tenth of a per cent or more. On a crowded band, two stations meant to be on separate channels drift on top of each other; a receiver tuned for a distant station loses it; a radio teleprinter (The Teleprinter) prints nonsense.
A quartz crystal fixes the frequency. A correctly cut plate of quartz in a simple circuit holds its frequency to about one part in 10,000 with no care at all, and to one part in a million in a box kept at a steady temperature. That gives you:
- Radio channels that stay put, so many stations can share the air and anyone can find them by dial setting alone (Radio).
- Frequency standards to calibrate every receiver and transmitter in a region.
- Quartz clocks that keep time to a fraction of a second a day — better than all but the finest pendulum clocks (The Mechanical Clock) — for Astronomy, Navigation and time signals sent by radio.
- The timing heart of every later The Computer.
How it works
Piezoelectricity
Squeeze a quartz crystal and electric charges appear on its faces: one face positive, the opposite negative. Pull it and the charges reverse. The reverse also happens: put a voltage across it and it squeezes or stretches very slightly. This is piezoelectricity ("pressure electricity"). The movement is tiny — a few millionths of a millimetre — but it is enough.
A bell that rings at one note
A plate of quartz, like a bell or a tuning fork, has a natural frequency at which it vibrates. For a thin plate vibrating through its thickness, that frequency depends almost only on the thickness: halve the thickness and the frequency doubles. Give the plate an electric push at its natural frequency and it rings strongly; at any other frequency it hardly responds.
To an electric circuit, the vibrating plate looks like an extraordinarily good tuned circuit. A good coil and capacitor have a Q (sharpness of tuning) of perhaps 100–200; a quartz plate has 10,000 to 100,000 or more. Put it in an oscillator in place of — or alongside — the tank circuit, and the oscillator is forced to run at the quartz's frequency and no other.
Quartz is ideal because it is hard, does not dissolve or absorb water, does not age, and — if cut at the right angle — its frequency barely changes with temperature.
Crystal axes and cuts
A quartz crystal grows as a six-sided prism capped by a point. Its behaviour depends on direction:
- The Z axis (optic axis) runs along the prism's length.
- The X axes (electrical axes) run across the prism from one corner (edge) of the hexagon to the opposite one. There are three.
- The Y axes run across the prism from the middle of one face to the middle of the opposite face.
A plate's behaviour depends on how it is cut from the crystal:
| Cut | How it lies | Frequency (thickness mode) | Change with temperature |
|---|---|---|---|
| X-cut | Faces square to an X axis | 2,860 ÷ thickness in mm, in kHz | About −20 parts per million per °C |
| Y-cut | Faces square to a Y axis | 1,960 ÷ thickness in mm, kHz | About +90 ppm per °C (poor) |
| AT-cut | Contains an X axis, tilted 35¼° from Z | 1,661 ÷ thickness in mm, kHz | Almost none near room temperature |
So a 1 MHz (1,000 kHz) AT-cut plate is 1.66 mm thick; a 3.5 MHz one is 0.47 mm; a 7 MHz one 0.24 mm. X-cut plates are the easiest first goal; AT-cut plates are what you want in the end.
What you need
| Item | Notes |
|---|---|
| Clear quartz crystals | At least 3–4 cm across, clear, without cracks (see below) |
| A slitting saw | Thin soft-iron or copper blade, in a frame or as a disc on a spindle, fed with wet grit — see Gem Cutting and Lapidary |
| Grits | Emery, garnet or crushed quartz sand, graded by settling into coarse, medium and fine (Abrasives and Grinding Stones) |
| Lapping plates | Two pieces of thick flat glass (Window Glass) or a flat cast-iron plate (The Blast Furnace and Cast Iron), 20 × 20 cm |
| A micrometer or thickness gauge | Reading to 0.01 mm (Measurement from Scratch, Scientific Instrument Making) |
| Brass sheet and springs | For the crystal holder |
| A triode and parts | Tube, RF choke, resistors, capacitors (The Vacuum Tube, Resistors, Capacitors and Coils) |
| A receiver | A regenerative receiver to hear and compare oscillators (Amplifiers and Oscillators) |
| For the demonstration | Cream of tartar from wine barrels, soda (Soda Ash and Baking Soda), foil |
Where to find it
- Rock crystal (clear quartz) grows in open cavities: in pegmatite veins in granite, in clefts in mountain rocks (the "crystal cellars" of the Alps), in geodes and in quartz veins. Look for hexagonal prisms with pointed ends, glassy, hard enough to scratch glass and steel, and not scratched by a knife (Rocks and Minerals). River gravels below such places sometimes carry broken crystals.
- Choosing a crystal: it must be clear, with no cracks, cloudy veils, bubbles or included needles in the part you will cut. Immerse it in a jar of clear oil (clove oil or any clear plant oil — Oils and Pressing); the outer surface nearly vanishes and you can see flaws inside. Smoky (brown) quartz works as well as colourless.
- Twinning: many crystals are in fact two crystals grown together with their axes turned, which spoils the plate. Some twins show as a zigzag seam on the faces, or as patches that look different in polarised light (look through the crystal between two "polarisers": each is a stack of 10–15 thin glass plates held slanting at about 57° to your line of sight, and the two stacks are turned at right angles to each other). Some twins cannot be seen at all and only show when a finished plate will not oscillate well. Expect to reject some plates.
- Cream of tartar for the Rochelle-salt demonstration is the hard crust (wine tartar) that grows inside barrels and vats where wine has stood (Beer, Wine and Cider).
Step 1: See piezoelectricity
Before cutting quartz, prove the effect to yourself with Rochelle salt, which is over a hundred times more strongly piezoelectric than quartz and easy to make.
- Scrape wine tartar from a barrel, dissolve it in boiling water, filter it through cloth, and let it cool: white crystals of cream of tartar form. Collect them.
- Stir 200 g of cream of tartar into 250 ml of boiling water — most of it will not dissolve yet. Stir in soda (sodium carbonate, Soda Ash and Baking Soda), a spoonful at a time. It fizzes. Stop when a new spoonful no longer fizzes. Filter while hot.
- Simmer to reduce it by about a third, then pour into a clean shallow dish and let it cool slowly, covered with a cloth, for a day or two. Clear crystals of Rochelle salt grow. Hang the best small one on a thread in fresh, just-saturated solution to grow it to 2–3 cm.
- Glue foil to two opposite faces. Connect the foils to an earphone. Tap the crystal with a pencil: the earphone clicks. Connect it instead to the output of an amplifier: it chirps faintly — it is now a loudspeaker.
- Connect it to a charged electroscope (Static Electricity and the Leyden Jar) and squeeze it in a clamp: the leaves move.
Rochelle salt dissolves in damp air, melts at 55 °C, and drifts. It is useless for frequency control — but it makes good earphones and microphones for Recording Sound.
Step 2: Orient and saw the crystal
- Hold the crystal so you can see its six prism faces. The Z axis runs along them.
- Mark the X axis you will use: a line across the end of the prism from one corner of the hexagon to the opposite corner. If the end is broken, look at the prism faces in cross-section, or grind a flat square across the prism to see the hexagon.
- X-cut plates: cut slices that run along the prism's length (parallel to Z) and lie at right angles to your X line. Each slice then has the X axis passing straight through its thickness.
- AT-cut plates: cut slices that contain the X axis (the X line lies flat in the slice) but are tilted 35¼° from the Z axis. Set the crystal in a block of pitch or plaster on the saw table, with the X axis horizontal across the blade and the Z axis tilted 35¼° from the blade's plane. A protractor made with Geometry and Trigonometry is accurate enough for a first try; each degree of error worsens the temperature behaviour.
- Saw with a soft-iron or copper blade fed with a slurry of medium grit and water (Gem Cutting and Lapidary). The grit, rolling under the blade, does the cutting. It is slow: about an hour per square centimetre of cut by hand. Slice plates about 0.3–0.5 mm thicker than the final thickness.
- Square each slice into a plate about 20 × 20 mm (or a disc 20 mm across), keeping a pencil arrow on it showing which way the X axis runs.
Step 3: Grind to frequency
- Make a flat: grind two glass plates face to face with medium grit, in figure-eight strokes, swapping which is on top every few minutes, until each is evenly grey all over. They are now flat.
- Rough grind: wet coarse grit on the plate, put the quartz on it, press with two fingertips spread over its whole face (or glue a cork to its back as a handle), and move it in figure-eights over the whole plate, turning it a quarter turn every few strokes. Do both faces.
- Measure the thickness at all four corners and the centre. Grind the thick side more until all five agree to 0.005 mm. A plate that is wedge-shaped will not oscillate, or will oscillate weakly at several frequencies.
- Finish with fine grit on a fresh plate, washing everything thoroughly when you change grits. One coarse grain left behind scratches the plate.
- Bevel the edges slightly on a fine stone; stray chips at the edges cause cracks.
- Wash with soap and water, then rinse in alcohol, and from now on touch it only by the edges. A fingerprint on the face can stop it oscillating.
- Test it in the oscillator (Step 5). Measure its frequency (Step 6). Then grind a little more, test again, and so on, creeping up on your target. You can only go up: grinding thinner raises the frequency. To pull it down slightly, rub a little soft pencil graphite over the middle of one face; the added weight lowers the frequency a few hundred hertz.
Work out roughly how much to take off: for an AT-cut plate, frequency in kHz × thickness in mm = 1,661. If a plate meant for 3,500 kHz is ringing at 3,480 kHz, it needs to be 1,661 ÷ 3,500 = 0.4746 mm instead of 1,661 ÷ 3,480 = 0.4773 mm: 2.7 thousandths of a millimetre more off — a few dozen strokes with fine grit.
Step 4: The holder
- Two brass plates 25 × 25 mm, lapped flat on the same glass plate as the crystal, polished, and cleaned.
- A small box of hardwood or shellacked fibre, with a brass spring pressing the top plate lightly on the crystal, and the lower plate fixed to the base. The crystal rests between them, centred, held only by light pressure.
- Better: set the top plate a hair above the crystal (an air gap of about 0.02–0.05 mm, a cigarette paper's thickness at most), with tiny spacers at the corners outside the quartz. The crystal then vibrates freely, and is more stable.
- Bring the plates out to two pins. Close the box against dust. Label it with the frequency and the cut.
Step 5: The crystal oscillator
The simplest circuit needs no tuning at all:
- Crystal from the tube's plate to its grid.
- Grid leak: 50–100 kΩ from grid to filament.
- Small capacitors: about 50–100 pF from grid to filament, and the same from plate to filament (Resistors, Capacitors and Coils). These, with the crystal, make the feedback loop.
- Plate supply: 90–150 V through a 2.5 mH radio-frequency choke.
- Output: take it from the plate through a 50 pF capacitor to the next stage (an amplifier stage, or the grid of a transmitter's power tube — see Amplifiers and Oscillators).
- Put a milliammeter in the plate supply. When the circuit oscillates, the plate current dips. To check, switch off, take the crystal out and switch on again: with nothing oscillating, the plate current is higher. (The holder's plates carry the full plate voltage; never touch them with the power on.)
For a transmitter, use the crystal oscillator only as a gentle master oscillator, and follow it with one or more amplifier stages. The crystal itself must never carry heavy current.
Frequency multiplying. A tube stage driven hard gives harmonics — two, three, four times the frequency. Tune that stage's plate circuit to the second harmonic and a 3.5 MHz crystal drives a 7 MHz transmitter.
Step 6: Measuring and matching frequencies
You need a reference. In a new network, choose one crystal as the master for the whole region and keep it in a steady-temperature box.
- Zero beat: run the master oscillator and the new crystal's oscillator side by side, both lightly coupled to a receiver. You hear a whistle whose pitch is the difference between the two frequencies. Grind the new crystal and the whistle falls in pitch; at a difference of a few hertz it becomes a slow flutter, and at zero it vanishes.
- Channels: for crystals at other frequencies, use harmonics. A 100 kHz master gives "markers" every 100 kHz up through the bands; grind each channel crystal to zero beat with a marker, or with a known fraction between markers measured on a calibrated receiver dial.
- Absolute time: the master's true frequency is found by running a quartz clock from it and comparing the clock with the stars over many days (Astronomy).
Step 7: Steady temperature and the quartz clock
The oven. A wooden box lined with felt, holding a smaller copper box with the crystal, a heating coil of iron wire, and a thermostat — a bimetal strip (brass riveted to iron) that opens a contact when it warms past a set point (Thermostats and Automatic Control). Set it to about 50 °C, above any room temperature, so it always heats and never needs to cool. With an AT-cut crystal in such an oven, the frequency holds to about one part in a million — about a tenth of a second a day if used as a clock.
The clock. A 100 kHz crystal oscillator is followed by divider stages — tube oscillators that lock to every tenth cycle of the stage before — giving 10 kHz, 1 kHz and finally a few hundred cycles a second. That drives a small synchronous motor (Synchronous Motors and Converters), whose speed is locked to the frequency, through gears to a clock dial. Later, transistor counters do the dividing (Electronic Counters). Expect ten or more tubes and many weeks of work. Build it once, for the observatory or the radio time-signal station, and set every other clock from its signals.
How to tell it worked
- The oscillator starts at once when switched on, the plate current dips, and a receiver finds a clean, steady whistle that does not shift when you wave your hand near the circuit or tap the bench.
- Warm the crystal holder with your hand for a minute: an X-cut plate's whistle moves a little; an AT-cut plate's hardly moves at all.
- Two stations each using their own crystal, ground to zero beat with the same master, can find each other day after day without retuning.
- A quartz clock in its oven, checked against star transits, gains or loses less than a second a week.
Note Troubleshooting. Will not oscillate → dirty faces (wash in soap, then alcohol); plate not parallel (measure the corners); holder pressing too hard; twin or crack in the plate. Try more plate voltage cautiously, or the other way up. Oscillates at two frequencies, or jumps → plate not flat, or the edges are chipped. Re-lap, bevel the edges, or cut a smaller square from the good middle. Frequency drifts a lot with warmth → cut at the wrong angle. An AT plate tilted the wrong way gives a large drift; cut the next ones tilted 35¼° the other way from Z. Plate cracked → too much plate voltage or a heavy load on the oscillator; keep the crystal stage gentle and drive the transmitter from a separate amplifier. Overshot the frequency → a dab of graphite pulls it down a little; otherwise relabel the crystal for a new channel and start another.
Dangers
Warning Quartz dust is a lung poison. Fine crystalline silica dust breathed over months causes silicosis, a scarring of the lungs that does not heal. Always saw and grind quartz wet, never dry; wipe up dried slurry with a wet cloth instead of sweeping it; and do the work in good ventilation.
- High voltage: the oscillator's plate supply (90–150 V) and any following transmitter stage (hundreds of volts) can kill. See Amplifiers and Oscillators and Wiring and Electrical Safety.
- Cuts: quartz breaks with razor edges. Handle broken crystals with gloves and grind sharp edges on chips.
- Oven heaters on a mains or battery supply can overheat if the thermostat sticks: fit a fuse and a second, higher-set safety contact.
What this unlocks
Fixed channels make radio orderly enough for a whole region's Radio network, radio teleprinters and data links (Networks and the Internet). Quartz clocks and radio time signals give everyone the same time to a fraction of a second, which is the basis of finding longitude at sea by radio (Navigation). Every The Computer runs from a crystal clock. Later steps:
- Synthetic quartz, grown from silica dissolved in hot alkaline water under high pressure in steel vessels (Pressure Vessels and Valves), ends the dependence on rare natural crystals.
- Piezoelectric ceramics, far stronger than quartz though less stable, for ultrasound, sonar and sensors (Piezoelectric Crystals and Ceramics).
- Atomic clocks, which check quartz against the vibration of atoms (Atomic Clocks (Overview)).
- Plating electrodes directly onto the crystal (silver by chemical silvering, as for Mirrors, or by evaporation in a vacuum) makes smaller, steadier crystals.
- Tuning-fork crystals at 32,768 Hz (2¹⁵) make small quartz watches possible once Integrated Circuits can divide the frequency down to one pulse a second.
How it was first done
The brothers Pierre and Jacques Curie discovered piezoelectricity in Paris in 1880, using quartz, tourmaline and Rochelle salt; Gabriel Lippmann predicted the reverse effect in 1881 and the Curies confirmed it the same year. Pierre Curie later used a quartz plate to measure tiny electric charges in Marie Curie's radioactivity research (Detecting Radiation). During the First World War Paul Langevin in France used quartz plates to send and receive underwater sound for detecting submarines. Walter Cady at Wesleyan University in Connecticut built the first quartz-controlled oscillators in 1921, and George Washington Pierce at Harvard devised the simple circuits still named after him in 1923. Warren Marrison and J. W. Horton at Bell Telephone Laboratories built the first quartz clock in 1927. The temperature-stable AT and BT cuts were found at Bell Labs in 1934. In the Second World War, tens of millions of crystals were cut and hand-finished from Brazilian quartz for military radios, much of the final grinding done by hand with abrasive on glass plates exactly as described here. Synthetic quartz came into wide use in the 1950s and 60s, and the first quartz wristwatch went on sale in Japan in 1969.
Source: content/entries/electronics/quartz-oscillators.md