Part 5 · Cloth and Clothing
Buttons, Buckles, Hooks and Zips
The small hard parts that open and close clothes — buttons of bone, horn, wood, shell and metal and the holes they go through, toggles, hooks and eyes, press studs, buckles and belts, safety pins, eyelets and grommets, laces, drawstrings and braces — and the zip, with its stamped teeth and the slider that locks them together.
- Difficulty
- ●●●●●
- Time
- A dozen bone buttons in an afternoon; a belt and buckle in a day; hooks, eyes and safety pins by the hundred once a jig is made; a working zip takes weeks of die-making
- Steps from zero
- 20 prerequisites →
This unlocks
—The full path from nothing — 20 steps before this one
- Cordage and Rope
- Fire
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Pottery
- Spinning and Weaving Cloth
- Horn and Bone Working
- Hides and Leather
- Sewing, Needles and Thread
- Bellows
- Iron (the Bloomery)
- Copper Smelting
- Blacksmithing
- Steel
- Copper Wire
- Iron and Brass Wire
- Buttons, Buckles, Hooks and Zips
Do them roughly in this order. See it on the tech tree →
Why it matters
A garment must open wide enough to get into and close snugly enough to keep warmth in. Without fasteners you are limited to things pulled over the head, wrapped and tied, or pinned with a thorn. With them you can make a coat that opens down the front, trousers that fit at the waist, baby clothes that change in seconds, a boot that laces tight and a pack that buckles to the body.
Fasteners are also the first mass-produced goods of many workshops: the punch and die that stamp buttons (Presses, Punches and Dies) go on to make coins and the Precision and Interchangeable Parts of machines.
Sewing, Needles and Thread already shows how to sew on a button and bind a buttonhole, and Horn and Bone Working how to cut button blanks. This chapter covers what is particular to each fastener.
How it works
Every fastener holds two edges together against a pull yet parts when you want. Something passes through a hole and turns (button, toggle, buckle tongue); a hook catches a loop (hook and eye, lace and eyelet); something springs into a hollow (press stud, safety pin, zip teeth); or a knot holds a cord (drawstring).
Two rules decide whether it works. The load must spread into the cloth: buttons and studs sit on a doubled edge backed by firm linen (a facing). It must survive washing: iron rusts, raw wood swells, horn softens in hot water, brass turns green (Laundry and Bleaching Cloth).
What you need
| Item | For | From |
|---|---|---|
| Bone, horn, antler, hardwood, shell | Buttons, toggles | Horn and Bone Working |
| Brass, iron or steel wire, 0.5–1.5 mm | Hooks and eyes, safety pins, springs | Iron and Brass Wire, Copper Wire |
| Brass sheet, 0.3–1 mm | Shank buttons, press studs, eyelets, zip parts | Sheet Metal and Rolling, Zinc and Brass |
| Pewter or brass | Cast buttons and buckles | Tin and Pewter, Metal Casting |
| Vegetable-tanned leather, 3–4 mm | Belts, brace tabs | Hides and Leather |
| Woven tape and webbing | Braces, zip tapes | Tablet and Band Weaving |
| Hollow punches, 2–30 mm | Cutting discs and holes | Iron tube sharpened inside and hardened (Steel) |
| A screw press | Stamping in quantity | Like the oil press of Oils and Pressing, with a heavy weighted bar across the top of the screw that is swung by hand |
Where to find it
- Bone from cattle leg bones and shoulder blades; horn tips for toggles, pressed horn sheet for flat buttons.
- Shell: thick freshwater mussels from clean gravel-bedded rivers, or oyster and abalone shells. You want a thick nacre — the rainbow-sheened inner layer.
- Hardwood: box, holly, hawthorn, apple, pear, olive, maple. Avoid oak in garments that get wet: its tannin stains black against iron.
- Coconut shell, ivory-nut palm seeds ("vegetable ivory") and antler also serve.
Buttons
Sizes and kinds
| Use | Diameter | Holes |
|---|---|---|
| Shirts, babies' clothes | 10–12 mm | 2 or 4, 1.5 mm, centres 3 mm apart |
| Waistcoats, cuffs, flies | 14–16 mm | 4, 1.5–2 mm |
| Jackets, braces buttons | 18–22 mm | 4, 2 mm |
| Coats | 22–30 mm | 4, or a shank |
| Coats worn with gloves | 30–40 mm, or toggles | Shank or cord |
A sew-through button has 2 or 4 holes and needs a thread shank wound under it (Sewing, Needles and Thread); a shank button has a loop on its back, better for thick cloth.
Bone, horn, wood and shell buttons
- Make a size jig: a hole through a hardwood block the exact size of the button. Every blank must drop through it; grind those that do not.
- Thickness: 3 mm for 12–15 mm buttons, 4 mm for 20 mm, 5 mm for coat buttons. Thinner bone cracks.
- Holes: mark them with a card template. Drill halfway from each side with a bow drill (Drills and Boring), then countersink each hole slightly with a bigger bit. Thread cut by a sharp hole is how most buttons are lost.
- Dish the face 0.5–1 mm with a broad rounded bit so the thread lies below the surface and does not wear.
- Polish a few hundred at once by tumbling them in a slowly turned barrel (Barrels and Cooperage) with wet sand and wood ash for a day, then dry bran.
Shell: cut blanks with a tube saw — an iron tube with teeth filed in its end, spun in a bow drill or The Lathe with water — and grind off the chalky outer layer on wet sandstone. Go slowly; keep it wet. Wood: turn a rod to the button diameter, cut the face profile every 5 mm along it, part each button off, drill, and boil in beeswax or linseed oil so it does not swell.
Thread and cloth buttons
- Dorset button: cover a 15 mm ring of wire or horn with tight blanket stitch, wind thread across it like wheel spokes, and weave round the spokes from the centre out. Light, washable, unbreakable.
- Knot button: a Chinese button knot or monkey's fist tied in 3–4 mm cord. With a cord loop, it makes a frog.
Metal buttons
Cast: pour pewter or brass into a two-part mould of stone, plaster or brass with 6–12 cavities on a channel (Metal Casting). For shank buttons, lay a short U of wire in a groove across each cavity first; the metal freezes round it.
Stamped (the industrial kind), from 0.3–0.5 mm sheet brass in a screw press: blank a disc; dome it in a second die (cupping stiffens thin metal greatly); blank and dome a smaller back with a central hole; push a splayed U of 0.8 mm wire through the back; then lay the back in the front and close the front's rim over it with a punch. The wire's feet are trapped inside.
Buttonholes and where they go
- Buttons sit on the centre line, not at the edge. The overlap from centre line to edge is the button's diameter plus 5–10 mm, so the edge never gapes.
- Horizontal buttonholes start 2–3 mm past the centre line towards the edge and run inward. Under strain the button slides to the end of the hole and stays on the line. Vertical holes, on a narrow shirt strip (the placket), are centred on the line.
- Spacing: one button at the fullest part of the chest, one at the waist, the rest evenly between — 7–10 cm apart on shirts, 10–12 cm on coats.
- Coats need a keyhole buttonhole: punch a 3 mm round hole at the edge end for the thick shank, and lay a thicker thread (gimp) along the slit before binding it so it cannot stretch.
- Back the cloth with a strip of firm linen 3–5 cm wide inside the front edge.
Toggles and loops
A toggle — a bar of wood, horn, bone or antler 3–6 cm long with a hole across the middle (Horn and Bone Working) — is sewn on by a short cord and pushed through a cord loop. It is the best closure for heavy coats and for people in mittens. Make the loop of 4–5 mm cord, just long enough that the toggle must be turned end-on to pass; sew both loop and toggle cord over a 4 × 6 cm patch of leather.
Hooks and eyes
A hook and eye closes edges that meet without overlapping: a dress back, a waistband, a collar. Bend them from brass or iron wire, 0.6–0.8 mm for dresses, 1–1.5 mm for coats and cloaks.
- Jig: three smooth iron pins in a hardwood block — two 2 mm pins 5 mm apart for the sewing loops, one 4 mm pin 10 mm in front of them for the bend.
- Hook: bend 45 mm of 0.7 mm wire double round the 4 mm pin; curl each leg out round its 2 mm pin into a sewing loop; then bend the doubled end back over itself with round-nose pliers into a hook with a 1.5 mm gap. Tap the hook flat so it holds stiffly.
- Eye: 30 mm of wire bent round the 4 mm pin into a U, feet curled into loops. A straight bar instead of a round eye suits edges that overlap a little.
- Tin iron hooks (Tin and Pewter) or they rust onto the cloth. Anneal brass if it cracks.
- Sew 5–6 stitches through each loop and 3–4 over the neck of the hook so it cannot tip. For a long opening, sew hooks 3–4 cm apart onto linen tape, then sew the tape in.
Press studs
A press stud (snap, popper) has a knob half and a socket half. Pushed together, the knob forces a spring in the socket open, passes it, and the spring closes behind the knob's widest part.
- Socket: blank a 10 mm disc of 0.3 mm brass and draw it into a cup 2 mm deep. Pierce a 3 mm hole in the bottom. Coil a split ring of 0.4 mm spring wire once round a 3.5 mm rod, lay it in the cup, and turn the cup's rim over it so it is trapped but free to open.
- Knob: blank the same disc and raise a knob 3.5 mm across and 2 mm high in its centre with a rounded punch into a matching die.
- Sewing holes: pierce four round each flange.
- Test: a pair should hold when the garment is shaken and part with a firm tug. Too stiff, open the ring a little; too loose, the knob is too small.
With no spring wire, cut the socket hole as a star of six slits; the tongues between them flex.
Buckles and belts
A buckle is a frame, a bar across it that the strap wraps round, and a tongue that pivots on the bar and passes through a hole in the strap. A roller on the frame's outer edge lets a tight strap slide without wearing.
Forged buckle: bend 5–6 mm iron rod hot into a rectangle or D, 5 mm wider inside than the strap, and weld or braze the joint (Blacksmithing, Soldering and Brazing). Forge the tongue from 3–4 mm rod, wrap its end round the bar, and round its tip so it cannot cut the strap. Cast buckles of brass or pewter are moulded like buttons, with the tongue added after.
Leather belt:
- Cut a strip of 3–4 mm vegetable-tanned leather along the backbone of the hide, where it stretches least: 25–30 mm wide for trousers, 40–50 mm for a work belt. Length: waist plus 20–25 cm.
- Bevel the edges, wet them and rub hard with a smooth bone until they shine (burnishing).
- Punch a slot 5 × 20 mm for the tongue 6–7 cm from the buckle end; fold the end round the bar and stitch or rivet it (Nails, Rivets and Wire Fasteners), trapping a keeper — a leather loop for the free end.
- Punch five holes, 4 mm, 25 mm apart; the middle one fits the wearer.
- Rub in tallow and beeswax (Footwear).
A woven belt (Tablet and Band Weaving) uses a slide buckle with a toothed bar, or two plain rings: thread the strap through both and back between them.
Safety pins
A safety pin is one springy wire: point, coil and guard.
- Hard-drawn brass or steel wire, 0.8 mm for a 35 mm pin, 1 mm for 50 mm, cut to twice the finished length plus 10 mm.
- Point one end on a fine whetstone before bending.
- Clamp the wire beside a 3 mm steel peg and wind one and a half turns round it, so the pointed leg crosses over the other.
- Bend the end of the plain leg back round a 2 mm pin into a hook for the point — or, better, crimp over it a little channel folded from thin brass sheet.
- Set the legs so the free point stands 5–8 mm from the guard; then it presses firmly home.
- Harden steel pins lightly (Springs): red heat, quench in oil, temper to blue.
Open and close each 20 times. If it stays open, the temper is lost.
Eyelets, grommets and laces
An eyelet is a small flanged metal tube lining a hole so a lace cannot tear it; a grommet is the larger two-piece version for canvas, a flanged tube plus a washer. (The rope ring sewn into sails, also called a grommet, is in Ropewalks and Sailcloth.)
- Draw a cup from a disc of soft brass 0.3–0.5 mm thick through two or three dies of shrinking size. A shoe eyelet ends up 4 mm inside and 3–4 mm long; a tent grommet 10–15 mm inside.
- Pierce the bottom, leaving the flange.
- Set it: punch a hole in the material slightly smaller than the barrel and push the eyelet through from the front. Stand it face-down on a hollow anvil and drive in a setting punch — a steel rod with a cone point inside a rounded shoulder. The cone splits the barrel; the shoulder rolls it over (onto the washer, for a grommet). The barrel must be 1.5–2 mm longer than the material is thick.
Laces are braided cords 2–4 mm thick (Cordage and Rope) or leather thongs (Footwear). Tip them with aglets: a strip of thin brass crimped round the end, or the last 2 cm dipped in hot glue or pitch and rolled hard between the palms as it sets.
Drawstrings
A drawstring runs through a casing — a channel sewn along a waistband or bag mouth, twice the cord thickness plus 5 mm wide. Bind the exit holes as eyelets, tack the cord at the centre back so it cannot pull out, and knot each end.
Braces
Braces (suspenders) hang trousers from the shoulders, so the waist can be loose — good for heavy work trousers and for children.
- Two straps of woven tape or soft leather 30–40 mm wide, each 110–125 cm long for an adult (front waistband over the shoulder to the back waistband, plus 15 cm).
- Cross them in an X at the back and sew them where they cross, or join them in a Y at a leather patch between the shoulder blades.
- Put a slide buckle on each front strap for length.
- End each strap in a leather tab with a buttonhole. They button onto six buttons inside the waistband: two each side at the front, 8–10 cm apart, and two at the back, 4–5 cm either side of the centre seam.
Elastic braces have threads of Rubber woven into the tape (Elastic and Rubber Thread).
The zip
The zip (zipper) is two tapes with rows of small metal teeth along their edges and a slider that pushes the teeth together so they lock, or wedges them apart. It is the hardest fastener here, because hundreds of tiny parts must be identical to a tenth of a millimetre. A rebuilding community will make buttons and hooks for years before zips, but the principle is simple and a first one can be made by hand.
How it works
- The tooth is a little scoop: a hollow pressed into its top face raises a bump underneath. Its back end splits into two legs that clamp round the tape edge.
- The tape is a strong woven band 12–15 mm wide with a thick cord (the bead) along its edge.
- Pitch: on each tape, the gap between teeth equals one tooth's thickness, so the other tape's teeth fit in the gaps.
- Locking: closed, each bump sits in the hollow of the neighbouring tooth from the other tape. Pulled sideways, every bump is held; the teeth can only part when the rows are bent at an angle, so the bumps lift out one at a time.
- The slider is a Y-shaped tunnel. Its two top mouths hold the rows apart at an angle; its walls converge so the teeth meet tilted and drop together one by one; the closed chain leaves straight at the bottom. Pulled back, a wedge between the top mouths forces the chain into a bend again, and the teeth unlock.
Making one by hand
Make a short zip first, 15 cm long, and expect failures.
- Weave two tapes (Tablet and Band Weaving) of hard-spun linen or cotton, 12 mm wide, with a 2 mm cord laid in along one edge.
- Flat wire: draw or roll brass to a strip about 5 × 1.5 mm (Iron and Brass Wire).
- Make three hardened steel tools (Machine Tools): a blanking punch and die that cuts a Y-shaped tooth 5 mm wide and 5 mm long from the strip; a forming punch and die that presses a hollow 1.5 mm across and 0.8 mm deep into the head; and crimping jaws that squeeze the legs onto the bead.
- Spacing jig: a steel bar with slots exactly 3 mm apart (1.5 mm tooth, 1.5 mm gap) holds the tape while each tooth is clamped on. Start the second tape half a pitch later than the first.
- Slider: cast it in brass in a two-part mould with a baked sand-and-clay core for the Y channel (Metal Casting), or build it from two 1 mm brass plates riveted to a central wedge. Each top mouth must be just wider than one tooth; the bottom throat just wider than the closed chain. File until it runs smoothly. Rivet on a pull tab.
- Stops: crimp a brass clip round the bead above the last tooth on each tape to keep the slider on, and one clip across both tapes below the first teeth to join them.
How to tell it worked
- Buttons do not move when pulled hard, and buttonholes survive 50 buttonings without fraying.
- Hooks do not open under a hard pull; press studs click shut and part with a firm tug but not when shaken.
- Buckles hold ten times the working load for a minute with no bent tongue or stretched slot.
- Zips stay shut when bent round a finger and pulled sideways; the slider runs smoothly both ways.
Note Troubleshooting. Buttons fall off → sharp holes cutting the thread, no shank, or thin cloth with no linen backing. Buttonholes gape → cut too long, or no gimp. Make them button width plus thickness plus 2 mm. Brown or green marks on cloth → rusting iron or corroding brass. Tin the parts, or wax them. Belt holes tear together → too close, or leather too thin or from the belly. 25 mm apart, 3–4 mm leather from the back. Zip splits behind the slider → the slider has spread; squeeze its walls slightly with pliers. A missing tooth always splits; replace it. Zip jams → a bent tooth, or tape caught. Straighten it; sew the cloth further from the teeth.
Dangers
Danger Small parts choke small children. Buttons, studs, beads and pins are the size a baby puts in its mouth and inhales. On children's clothes, sew buttons with doubled thread through every hole and check them at every wash; prefer large toggles or firmly sewn studs. Keep safety pins away from a baby's face, closed and pointing away from the body, and count them.
Danger Cords round children's necks strangle. No drawstrings in children's hoods or necklines, no long cords on toggles, no mitten strings round the neck. Hood cords catch on slides, gates and branches, and children have died that way (Making Clothes).
- Presses crush fingers. A screw press with a weighted bar delivers several tonnes. Feed blanks with tongs or a slide, never by hand, and keep your head clear of the swinging bar.
- Hardened punches chip and fly when struck. Shield your eyes.
- Brass fumes cause metal fume fever (Zinc and Brass); cast outdoors. Never put lead in children's buttons.
What this unlocks
- Fitted clothes (Making Clothes), waterproofs (Raincoats, Oilskins, Umbrellas and Rubber Boots), gloves and caps (Hats, Gloves, Scarves and Stockings).
- The hardware of Bags, Backpacks, Wallets and Luggage, Tents, Sleeping Bags and Camping Gear and pack harness.
- The press and dies go on to coins (Money, Trade and Record-keeping), lock parts (Locks and Keys) and The Sewing Machine parts.
- Casein and Bakelite buttons (Early Plastics), nylon coil zips (Rayon and Nylon), and clasps and chains (Jewellery, Beads and Medals).
How it was first done
People closed clothes with thorn and bone pins, ties and belts long before buttons, and early buttons in Bronze Age graves were mostly ornaments. The fibula, a bronze brooch with a coiled spring and a catch that hides the point, was made in Europe from about 1300 BC — the ancestor of the safety pin. Romans fastened belts with cast bronze buckles.
The buttonhole spread in Europe in the 1200s and made close-fitting clothes possible. In the 1700s and 1800s Birmingham in England stamped buttons by the million on hand screw presses. John Boepple started the American pearl-button industry from river mussel shells at Muscatine, Iowa, in 1891.
Walter Hunt of New York patented the safety pin in 1849 and sold the rights for 400 dollars. Heribert Bauer patented the press stud in Germany in 1885. The zip began as Whitcomb Judson's clumsy "clasp locker" of 1893; Gideon Sundback, a Swedish-born engineer in the United States, made it work in 1913 with nesting cupped teeth, and by 1917 had a machine that stamped teeth from flat wire and clamped them onto the tape. The B. F. Goodrich company named it the "zipper" in 1923, for its rubber galoshes (Raincoats, Oilskins, Umbrellas and Rubber Boots).
Source: content/entries/textiles/clothing-fasteners.md