Jewellery, Beads and Medals

Small, fine metalwork that lasts for centuries — rings and signet rings, chains and necklaces, earrings, bracelets, brooches and their clasps, beads of shell, stone, glass and metal, and stamped or cast medals and badges. It is also where you learn to solder tiny joints, cast in lost wax at fingertip scale and set stones so they never fall out.

Difficulty
●●●●●
Time
An afternoon for a plain ring or a string of shell beads; a day for a soldered chain or a set stone; a week to carve, invest and cast a signet ring
Steps from zero
17 prerequisites →

You need first

Gold and SilverGem Cutting and LapidaryMetal Casting

This unlocks

—
The full path from nothing — 17 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Abrasives and Grinding Stones
  11. Hides and Leather
  12. Gem Cutting and Lapidary
  13. Bellows
  14. Copper Smelting
  15. Lead
  16. Gold and Silver
  17. Metal Casting
  18. Jewellery, Beads and Medals

Do them roughly in this order. See it on the tech tree →

Why it matters

Jewellery is the oldest made thing that is not a tool: people strung shell beads more than 100,000 years ago, before they had pots. It is more than decoration. A gold ring or silver chain is savings you can wear and trade anywhere (Money, Trade and Record-keeping). A signet ring pressed into warm sealing wax signs a letter or contract. Medals and badges show who did a brave deed or holds an office. The skills — soldering a 1 mm joint, filing a hinge true — are the same ones that make instrument and watch parts (Scientific Instrument Making, Watches and Small Clocks).

This chapter assumes you can win and refine the metals (Gold and Silver, Copper Smelting, Zinc and Brass), cast in lost wax (Metal Casting), draw wire (Iron and Brass Wire) and polish stones (Gem Cutting and Lapidary). It covers what is particular to small, worn things.

How it works

Metal hardens as you bend it and softens when you heat it. Every bend and blow makes silver, gold, copper and brass harder and springier, until it cracks. Annealing — heating to a dull red (about 600–650 °C, just visible in a shaded room) and quenching in water — makes it soft again. Anneal to shape; let the last few blows work-harden the piece so a ring keeps its round and a pin its spring.

Solder flows to the hottest clean metal. Hard solder (Soldering and Brazing) is drawn into a joint by capillary action only if the joint is clean, fluxed, closed with no visible gap, and both sides reach flowing heat together. On small work, heat the whole piece and the solder follows the heat. For pieces with several joints use graded solders: hardest first, softer later, so early joints do not reopen.

Pure metals are too soft to wear. Alloy them (Gold and Silver):

Alloy Make-up Melts Use
Fine silver 99.9% silver 961 °C Bezels (soft, easy to push over a stone)
Sterling silver 925 silver : 75 copper about 800–890 °C Rings, chains, almost everything
22 karat gold 22 gold : 1 silver : 1 copper about 1,000 °C Rich, soft — wedding bands
18 karat gold 18 gold : 3 silver : 3 copper about 900 °C Best all-round gold for rings and settings
Copper, brass, bronze Zinc and Brass, Bronze 900–1,080 °C Practice pieces, badges, medals

What you need

Tool How to get or make it
Charcoal block Dense charcoal 10 × 15 × 4 cm, sawn flat; reflects heat and stops oxidising (Identifying Substances)
Blowpipe and lamp A brass tube 20–25 cm long, tapering to a 1 mm tip, blown into an oil-lamp flame — the old goldsmith's torch. A small bellows or a gas torch is easier
Jeweller's saw A steel frame 10–15 cm deep holding a blade under tension. Blades from hardened clock-spring 0.3–0.5 mm thick, 20–30 teeth per cm (Files and Saws)
Needle files, pliers Small files 12–16 cm; round-nose, flat-nose and half-round pliers with smooth jaws, forged from Steel
Ring mandrel Tapered, polished steel or hardwood rod 25–30 cm long, 10 mm to 26 mm across
Mallet Rawhide, horn or boxwood — shapes without marking
Dapping block Hardwood or brass block with hemispherical hollows 4–25 mm across, and round-ended punches to match
Burnisher, pusher, gravers Polished hardened steel tongue; blunt square rod in a handle; small square and lozenge steel chisels for engraving
Pickle pot Warm alum solution (a handful per litre — Dyes and Mordants) or 10% Sulfuric Acid; copper tongs only
Polish Tripoli and rouge (Abrasives and Grinding Stones) on leather sticks or a soft wheel on a The Lathe

Where to find it

Shells come from beaches and river banks: thick pearly shells (mussel, oyster, abalone, freshwater clam) give mother-of-pearl; small whole snail shells (dog-whelk, cowrie) only need a hole. For casting investment you need plaster (Gypsum and Plaster of Paris) and very fine quartz flour (quartz heated red, quenched, crushed and settled — Abrasives and Grinding Stones).

The basic skills

  1. Sawing. Fit the blade teeth pointing down toward the handle, squeezing the frame slightly so the blade is tight and "pings" when plucked. Saw with long, light strokes.
  2. Annealing. Heat evenly on the charcoal to dull red; quench silver and copper in water; let gold cool to black heat first.
  3. Soldering. File the joint until no light shows through. Paint it with borax paste. Cut solder into pallions about 1 × 1 mm and lay one across the joint. Heat the whole piece gently until the borax settles to glass, then to an even dull-cherry red, flame moving. The solder suddenly flashes into the joint as a bright line: stop at once.
  4. Pickling. Drop the warm piece into pickle for 5–15 minutes until it comes out white or matte; rinse.
  5. Finishing. File, rub with abrasive paper from 400 to 1,200 grit, polish with tripoli, finish with rouge. Rubbing an edge hard with the burnisher gives a mirror shine with no loss of metal.

Solders. Melt fine silver with brass on charcoal under borax and hammer the button into thin sheet:

Grade Silver : brass by weight Flows at about Use
Hard 4 : 1 780 °C (cherry red) First joints — ring seams, bezels
Medium 3 : 1 750 °C Second joints
Easy 2 : 1 720 °C (dull red) Last joints, repairs, ear posts

For gold, melt some of your gold with up to an equal weight of hard silver solder. Never use solder containing cadmium (see Dangers).

Rings

Plain band

Size. Inside diameters run from about 15 mm (small woman's finger) to 22 mm (big man's). Measure with a paper strip round the base of the finger and check it passes the knuckle. A ring should go over the knuckle with a firm push and turn on the finger without pinching.

Blank length. Metal stretches outside and squeezes inside, so measure the middle of the thickness:

blank length = (inside diameter + metal thickness) × 3.14

For an 18 mm ring of 1.5 mm strip: (18 + 1.5) × 3.14 = 61.2 mm. A comfortable band is 2–6 mm wide and 1.2–2 mm thick.

1. Cut the blank 2. Bend, ends tight 3. Solder the seam 4. True on mandrel length L L = (D + t) × 3.14 D = inside diameter t = metal thickness 18 mm ring, 1.5 mm strip: L = 61.2 mm file ends square seam push ends past each other and back so they spring shut by themselves. No light through the joint. solder chip on seam blowpipe flame charcoal block heat the whole ring evenly to dull-cherry red tapered mandrel rawhide mallet tap it round; turn the ring over halfway because the mandrel tapers
Fig. 1 Making a plain ring. Cut a blank to the calculated length, bend it into a hoop with the ends meeting tight, solder the seam on the charcoal block, then true it round on the tapered mandrel with a rawhide mallet.
  1. Cut the strip to length; file both ends square. Anneal.
  2. Bend it round with half-round pliers or around the mandrel. Push the ends past each other and back, so they spring together flat and tight on their own — a ring held closed by hand springs open in the heat.
  3. Hold it to the light: no light through the seam. File until none shows.
  4. Flux, place one pallion of hard solder inside the seam, and solder with the ring standing on edge on the charcoal.
  5. Pickle, slide it on the mandrel and tap it round with the mallet, turning it over halfway (the mandrel is tapered).
  6. File off extra solder, round the inside edges for comfort, polish.

Good or bad. A good ring is perfectly round, shows no seam, is the same width all round and sits flat on a table. A dark line in the seam means missing solder; a lump inside rubs the finger.

Signet ring

A signet ring has a thick flat head (10–15 mm long, 8–12 mm wide, 3–4 mm thick) carrying a design cut in reverse and sunk in, so that pressed into warm wax it leaves a raised, right-reading seal. It is cast in lost wax (Metal Casting) at small scale:

  1. Carve the model in hard wax (3 parts beeswax : 1 part pine resin, a pinch of soot to show detail). Shank 1.5–2 mm thick at the back, thickening into the head. Leave the face blank.
  2. Sprue it: a wax rod 3–4 mm thick, 10–15 mm long, from the back of the head (the thickest part) to a cone that becomes the pouring cup. You need about 11 times the wax weight in sterling silver, or 16–20 times in gold (more for higher karat), plus 30% for sprue and cup.
  3. Invest it. Stand the model cup-down in a short iron tube (the flask) 4–6 cm across, 1 cm clear all round. Mix 1 part plaster : 1 part fine quartz flour by weight with about 40 parts water per 100 of powder. Brush a first coat on the model to drive off bubbles, fill the flask, and tap it for a minute.
  4. Burn out after 2 hours: cup-down in a The Kiln or embers, rising over 3–4 hours to dull red (about 700 °C), held an hour until the cup glows clean. Above about 730 °C the plaster breaks down and stains the metal.
  5. Steam cast. Let the flask fall to about 500–600 °C (the faint red just gone) and set it cup-up in dry sand. Melt the metal well past its melting point — sterling bright orange and spinning freely. Pour, and at once press over the cup a jar lid packed with a 1 cm wad of wet cloth or leather. The steam drives the metal into every detail; without that push, small work often freezes before it fills.
  6. After 5 minutes plunge the flask into water; the plaster bursts away. Pickle.
  7. Engrave the face in reverse with gravers (Engraving, Seals and Etching), checking by pressing into soft wax as you go. Start with initials and a border.

A good signet gives a crisp, right-reading seal with no bubbles in the field. A rough, pitted surface means wet investment, a dirty burnout or overheated metal; a half-filled shank means the flask or metal was too cold.

Chains, necklaces and bracelets

Chain

  1. Wind a coil. Anneal wire 0.8–1.2 mm thick (1.5–2 mm for a strong chain) and wind it turn against turn round a smooth steel rod 3–6 mm across, clamped in a vice and turned by a crank.
  2. Saw lengthwise along the coil: each turn drops off as an open jump ring with flush ends.
  3. Join. Open each ring by twisting the ends sideways (pulling them apart spoils the round), pass it through the last link, and twist it shut, flush and tight.
  4. Solder each link on the charcoal with a pallion of easy solder and a small pointed flame, doing every second link, then turning the chain to do the rest.
  5. Pickle, pull the chain through a hole in hardwood to even the links, and polish by tumbling it for a few hours with soapy water and small hard gravel.

A good chain hangs without kinks, every link moves, and none opens under the hardest two-handed pull you can give it.

Necklace

A chain or string of beads with a clasp: 40–45 cm sits at the base of the neck, 50–60 cm falls to the breastbone, over 70 cm passes over the head without a clasp. String beads on doubled waxed silk or flax (Silk, Flax, Hemp and Linen) with a knot between every bead, so a broken thread loses one bead and beads do not rub each other.

Bracelet

  • Bangle: a closed hoop of 3–5 mm wire or 1.5 mm strip, 60–70 mm inside (measure round the knuckles with the thumb tucked in), made and soldered like a ring.
  • Cuff: an open oval band 10–30 mm wide with a 25–30 mm gap, pushed on sideways; planish it (light overlapping blows on a polished stake) so it springs back.
  • Chain bracelet: 17–20 cm of chain with a clasp.

Clasps, earrings and brooches

These small working parts — jewellers call them findings — fail more than anything else. Make them of work-hardened wire and test them.

Coil and jump rings Soldered chain Hook clasp Toggle clasp Ear wire Brooch (back) saw along here wire wound on a 3–6 mm rod open rings with flush ends soldered seam twist ends sideways to open; thread through the last link, close tight, solder every link 1–1.2 mm hard wire, 10–15 mm long, curve hammered flat; hooks into a soldered ring bar ≥ ring + 4 mm bar joined at its middle; it cannot pull back through 0.8 mm wire, about 4 cm end smooth, rounded, burnished loop for the drop hinge pin catch set near the top; catch opens downward; pin 0.9–1.2 mm, hard
Fig. 2 Findings. A coil wound on a mandrel and sawn into jump rings; a soldered chain; a hook clasp and a toggle clasp; an ear wire; a brooch with hinge, pin and catch.

Clasps

  • Hook: 1–1.2 mm hard wire bent into an S or J 10–15 mm long, the curve hammered slightly flat to stiffen it, hooking into a soldered ring. Good on a hanging necklace; can slip off a loose bracelet.
  • Toggle: a ring 10–15 mm across on one end, a bar on the other, joined at its middle by two or three links. The bar must be at least 4 mm longer than the ring's inside diameter. It cannot open under pull.

A good clasp holds a 2 kg weight hung from it and shaken.

Earrings

  • Ear wire: 0.8 mm wire about 4 cm long, bent into a shepherd's hook with a loop for the drop. File and burnish the end that goes through the ear smooth and rounded.
  • Stud: a post 0.8 mm thick and 10–12 mm long soldered upright on the back with easy solder, held by a friction ear nut (a small disc with two curls of sheet gripping the post).
  • Hoop: 0.8–1.2 mm wire, one end filed to a blunt point, the other bent into a catch loop.

Use only fine silver, sterling, 14 karat gold or better, or pure titanium (Titanium) for anything through skin. Copper and brass stain and cause sores; nickel causes allergies. Boil earrings in soapy water before wearing, and pierce ears only with a sterilised needle (Sterilising Instruments and Dressings).

Brooches and pins

A brooch is a decorated plate with a pin behind it and a catch to hold the point.

  1. Make the front: a disc, a cast piece, an enamelled plate (Enamel on Metal) or a set stone.
  2. Solder a hinge (two small lugs with a cross wire, or a short tube) and a catch (a small hook of sheet opening downward, so gravity keeps the pin in) on the back with medium solder, near the top edge so the brooch does not tip forward.
  3. Make the pin of hard wire 0.9–1.2 mm thick, 2–3 mm longer than the hinge-to-catch gap. Work-harden it by twisting and light hammering, file a long smooth taper and polish the point. It should spring into the catch.

The ancient fibula — the first safety pin — is all of this in one bronze or brass wire: point, a coiled spring of two or three turns, a bow, and a catch bent up at the far end. It is a one-hour first brooch.

Setting stones

Stones come from Gem Cutting and Lapidary or Synthetic Gems. A setting must hold the stone so it cannot fall out, rattle or grind against the metal.

Bezel setting (cabochon) Claw setting (faceted stone) cabochon bezel fine silver 0.3–0.4 mm, rubbed over girdle widest part base plate Bezel rises at least 1 mm above the girdle. Push N, S, E, W, then between; burnish. Best for soft stones: shell, amber, opal. faceted stone claw tip bent over, 1 mm high seat notch claw 0.8–1 mm collar 4 or 6 claws; seats cut at one height just below the girdle.
Fig. 3 Two ways to hold a stone. A bezel is a thin wall of fine silver soldered to a base and rubbed over the edge of a domed cabochon. Claws are wire posts that rise beside a faceted stone, hold it in notches cut just below its widest edge, and are bent over its top.

Bezel (for cabochons).

  1. Use fine silver or 22 karat gold strip 0.3–0.4 mm thick, tall enough to rise at least 1 mm above the stone's widest edge (its girdle) — usually a quarter to a third of the stone's height.
  2. Wrap it snugly round the stone, cut, and hard-solder the seam. The stone must drop in with no wobble; stretch a tight bezel on a tapered stake, or cut and re-solder a loose one.
  3. Solder it to a base plate or ring head with medium solder; saw off the extra plate.
  4. Drop in the stone. Press the bezel in with the pusher at north, south, east, west, then between them, a little at a time. Pushing all round one side makes pleats.
  5. Burnish the edge until it lies tight and shiny on the stone.

Claws (for faceted stones).

  1. Solder 4 or 6 claws of 0.8–1.0 mm wire evenly round a ring of wire slightly smaller than the stone's girdle.
  2. With a graver cut a notch (seat) inside each claw at exactly the same height, just below the girdle.
  3. Snap the stone into the seats, level.
  4. Push the claws over the stone, opposite pairs first; trim to 1 mm above the girdle, round and polish.

A good setting gives no rattle when shaken by your ear and no gap a fingernail can enter. Soft stones (shell, amber, opal) go only in bezels; claws crack them.

Beads

Stone beads are drilled as in Gem Cutting and Lapidary; glass beads are wound on a clay-coated rod as in Glass.

  • Shell beads. Break thick shell into squares 6–10 mm across. Drill each from both sides with a bow drill (Drills and Boring) and a flint or steel point, wet — a minute or two each. Thread 20–50 tightly on a stiff cord and roll the whole string on wet sandstone until all are ground to one even round disc. Polish on leather with chalk.
  • Metal beads. Dome two discs of 0.4–0.5 mm sheet in the dapping block, file the rims to meet, drill a 1–1.5 mm hole in each, and solder them together. Always leave the holes open: trapped air expands and bursts the joint.
  • Clay beads. Roll fine clay balls, pierce with a stem or wire, dry and fire with pots (Pottery); glaze if you like (Glazes).

Holes of 1–1.5 mm suit silk; 2 mm or more for leather thong. A good bead has a smooth hole at both ends that will not cut the thread.

Medals and badges

A medal is a disc with a design in relief, given to honour a person or event and hung from a ribbon. A badge is a smaller piece worn on the clothes by a pin or loop, to show rank, office or membership.

  • Struck medals and badges are made like coins, with a pair of hardened steel dies (Money, Trade and Record-keeping, Steel). Use annealed blanks 30–40 mm across and 2–4 mm thick of copper, bronze or silver; strike, anneal and strike again, two to four times for a deep design. A screw press (Screws, Nuts and Bolts) gives much crisper work than a hammer. Drill the rim or solder on a loop, add a jump ring and a ribbon 25–35 mm wide.
  • Cast medals need no dies: model the design in wax on a flat disc, or press a carved original into fine green sand (Metal Casting), and cast in bronze or brass. Sharpen the detail afterwards with gravers and small chisels (chasing).
  • Stamped badges: lay a blank of copper or brass sheet 0.5–0.8 mm thick on a block of lead or pitch and drive a steel punch carrying the raised design into it with one heavy blow. Fill hollows with enamel (Enamel on Metal) for colour; solder a pin and catch behind.

A good medal or badge has sharp detail right to the edge, no cracks at the rim, a flat field, and a loop or pin strong enough to hang 1 kg.

How to tell it worked

  • Rings round and seamless; a band does not bend when squeezed hard between finger and thumb.
  • Solder joints are smooth fillets with no gaps or lumps. Grey, crumbly joints were overheated.
  • Chains survive a hard two-handed pull; clasps survive the 2 kg shake; settings do not rattle.
  • Precious metal is the right colour and weight and passes the touchstone (Gold and Silver). Stamp every piece with a small punch giving its fineness and maker — a hallmark — so buyers can trust it.

Note When it goes wrong. Solder balls up and will not flow → dirty joint, burnt-out flux, or the piece is not hot all over. Pickle, re-flux, heat the whole piece. Solder runs everywhere but the joint → gap too wide, or one side hotter. Close the joint; heat the heavier part first. Earlier joints open → same solder used twice. Use a lower grade, or paint old joints with rouge paste. Grey stain under the polish on sterling (firescale) → copper oxidised under the surface. Coat with borax before every heating, or polish it away.

Dangers

Danger Cadmium. Some old and bought silver solders contain cadmium. Its fumes, given off silently by overheated solder, can destroy the lungs and kill within days. Make solder from silver and brass only, and work in moving air.

Danger Rings and machinery. A ring caught on a machine, rope or ladder can strip the flesh off a finger or tear it off. Remove rings, bracelets and necklaces before working with machines, ropes, animals or heavy loads. Cut a ring off a swollen or injured finger at once.

  • Molten metal for casting spits violently on anything damp. Dry and warm every tool, flask and mould; wear eye protection and leather; see Metal Casting.
  • Small children choke on beads, earring backs and charms. Keep them out of reach.
  • Pickle and acid burn eyes and skin; cover your eyes and add acid to water, never the reverse (Acids, Bases and Testing).
  • Mercury gilding (gold dissolved in mercury and the mercury burnt off) poisons the worker and the neighbours. Gild by Electroplating instead.

What this unlocks

The same hands make the fine parts of Scientific Instrument Making and Watches and Small Clocks; precious-metal contacts serve the The Telegraph and Radio. Seals and medals carry the trust that Money, Trade and Record-keeping and Organising a Community depend on. Buttons and buckles are close cousins (Buttons, Buckles, Hooks and Zips). Synthetic Gems and anodised Titanium (Anodising Aluminium and Titanium) add new colours.

How it was first done

The oldest known beads are pierced sea-snail shells stained with ochre, from Skhul and Qafzeh in Israel and from North Africa, about 100,000 years old; from Blombos Cave in South Africa, about 75,000. Gold rings, bracelets and beads lie in the cemetery at Varna, Bulgaria, from about 4500 BC. The royal tombs of Ur (about 2600 BC) hold soldered gold and carnelian necklaces and woven loop-in-loop chain. Signet rings and engraved seals signed documents in Mesopotamia and Egypt for thousands of years. Bronze Age Europe invented the fibula around 1300 BC; the Etruscans perfected granulation — tiny gold grains fused to gold sheet — in the 7th century BC. Pisanello revived the cast portrait medal in Italy around 1438–1440.