◆ Rebuild

Part 2 · Earth and Fire

Fused Quartz and Halogen Lamps

Pure silica melted into glass hardly expands when heated, so it can go red-hot into cold water without cracking, stands 1,100 °C for years, and lets ultraviolet light through. How to melt it from rock crystal in an oxy-hydrogen flame or from sand around an electrically heated carbon rod, how to work quartz tube and make crucibles, and how a quartz envelope and a pinch of bromine make the bright, long-lived tungsten-halogen lamp.

Difficulty
●●●●●
Time
An afternoon to fuse quartz rod in a flame once you have oxygen and hydrogen; a few weeks to set up electric fusion of tube; months of practice for foil seals and working halogen lamps
Steps from zero
34 prerequisites →

You need first

Scientific Glassblowing and Glass-to-Metal SealsTungsten and Filament Wire

This unlocks

—
The full path from nothing — 34 steps before this one
  1. Fire
  2. Stone Tools
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. The Kiln
  9. Pottery
  10. Charcoal
  11. Hides and Leather
  12. Lime
  13. Salt
  14. Mercury
  15. Lye and Potash
  16. Fermentation
  17. The Wheel and Axle
  18. Glass
  19. Bellows
  20. The Lathe
  21. Copper Smelting
  22. Iron (the Bloomery)
  23. Laboratory Glassware
  24. Pumps
  25. Blacksmithing
  26. The Vacuum Pump
  27. The Battery
  28. Scientific Glassblowing and Glass-to-Metal Seals
  29. Steel
  30. Electrolysis
  31. Copper Wire
  32. Iron and Brass Wire
  33. Hydrogen, Oxygen and Gases
  34. Tungsten and Filament Wire
  35. Fused Quartz and Halogen Lamps

Do them roughly in this order. See it on the tech tree →

Why it matters

Ordinary glass softens at 600–800 °C and cracks if heated or cooled suddenly (Glass). Borosilicate does better (Scientific Glassblowing and Glass-to-Metal Seals). Fused quartz — silica alone, with nothing added — is in a class of its own:

  • It barely expands — about 0.55 millionths per degree, a sixth of borosilicate — so a red-hot quartz tube can be dropped into cold water and survive.
  • It works for years at 1,000–1,100 °C, for hours at 1,200 °C.
  • It passes ultraviolet that ordinary glass blocks.
  • It is pure and inert; only hydrofluoric acid, hot phosphoric acid and hot alkalis attack it.

That makes it the material of furnace tubes for making silicon and chips (Pure Silicon, Making Microchips), crucibles for growing crystals, mercury and ultraviolet lamps (Arc Lamps, Neon and Fluorescent Lights, Sterilising Instruments and Dressings), optical fibre (Fibre Optics), thermocouple sheaths, sight glasses for hot furnaces, and the small, hot envelope of the halogen lamp.

How it works

Crystal to glass. Quartz is crystalline silica. Heated, it changes shape inside at 573 °C with a sudden small jump in size (which is why quartz pebbles shatter in a fire), and further changes higher up. It melts at about 1,713 °C — but the melt is unbelievably thick, like cold tar even at 2,000 °C. Cool it and the atoms never find their places again: it freezes as a glass, fused quartz (also called fused silica or quartz glass).

Bubbles stay in. Because the melt is so thick, air between grains cannot rise out. Melted sand becomes white, milky translucent quartz, full of tiny bubbles: excellent for tubes, crucibles and muffles, but not for windows. Clear quartz needs clean crystal, melted a little at a time so each grain's air can escape, in a flame or in a vacuum.

Devitrification. Above about 1,100 °C, the glass slowly tries to turn back into crystal (called cristobalite). It starts at the surface as a white, frosty skin, and is hugely speeded up by sodium and potassium — the salts from a single fingerprint. On cooling below about 250 °C, the frosty skin shrinks suddenly and flakes, and the tube may crack. So quartz must be clean before it is heated, and kept below 1,100 °C in long service.

Working range. Quartz begins to soften at about 1,650 °C and is worked at 1,800–2,000 °C — far hotter than any glass. It needs an oxygen–hydrogen or oxygen–gas flame (Hydrogen, Oxygen and Gases). At those heats a little silica evaporates and settles as a white flame deposit of fine powder near the hot zone.

What you need

Item Notes
Quartz Clear rock crystal for clear quartz; white vein quartz or the purest white sand for translucent (Rocks and Minerals, Glass)
Acids Hydrochloric acid to clean the grain (Hydrochloric Acid)
Oxygen and hydrogen (or fuel gas) In separate holders or cylinders with flashback arrestors (Hydrogen, Oxygen and Gases, Liquid Air, Nitrogen and the Noble Gases)
Graphite Electrode stock for rods, moulds and paddles (The Electric Arc Furnace)
Electric power A heavy low-voltage transformer for electric fusion (The Transformer, Welding)
Very hot furnace For crucibles and annealing (Very-High-Temperature Furnaces)
Molybdenum Foil 0.02–0.03 mm thick and wire, made like tungsten from molybdenite (Molybdenum)
Tungsten Coiled filaments (Tungsten and Filament Wire)
Krypton or argon, bromine or iodine Lamp fills (Liquid Air, Nitrogen and the Noble Gases, Bromine and Bromides, Iodine)
Vacuum pump For lamps (The Vacuum Pump)
Welding glass Shade 5–6 for working quartz (Welding)

Where to find it

Rock crystal — water-clear quartz in six-sided crystals with pointed ends — grows in cavities and veins in granite and in mountain rocks, and is found as rounded clear pebbles in some rivers. It scratches glass, cannot be scratched by steel, and breaks with curved, shell-like faces. White vein quartz is the same mineral, milky with tiny bubbles of fluid; it is common in veins through slate and granite country. Pure white sand is mostly quartz grains (Glass). Reject any with rust stains, dark grains or mica.

Preparing the grain

  1. Crackle it. Heat lumps of quartz to red heat (about 800 °C, well past the 573 °C jump) and drop them into cold water. They craze through and crumble easily.
  2. Crush and sieve to the size you need (Ball Mills, Crushers and Grinders): 0.1–0.3 mm for flame fusion, 0.2–1 mm for electric fusion. Crush between quartz or flint, not iron, if you can; if not, pull out iron with a magnet.
  3. Pick. For clear work, spread the grain on a dark cloth and pick out any grain that is cloudy, coloured or dark.
  4. Wash in warm dilute hydrochloric acid for a day to dissolve iron stains, then rinse many times in rain or distilled water (Distillation). Dry in a clean oven. From now on, touch it only with clean tools.

Method 1: Flame fusion — clear rod and small tube

Flame fusion Clean grains0.1–0.3 mm Oxy-hydrogenburner Clear lump turn, draw back Then: draw into rod2–6 mm, or work into tube Electric fusion Fused sleeve3–8 mm wall, translucent Pure sand10 cm all round Graphite rodwhite-hot 10–30 V, 500–2,000 A Firebricktrough in section: rod,sleeve, sand
Fig. 1 Two ways to fuse quartz. Left: flame fusion. Clean crystal grains fall slowly into an oxy-hydrogen flame and melt onto the end of a turning quartz rod, which is drawn back as it grows; the clear glass can be pulled into rod or worked into tube. Right: electric fusion. A graphite rod buried in a trough of pure sand is heated white-hot by a heavy current; a layer of sand fuses round it, and when the rod is pulled out a tube of translucent quartz remains.

This is the way clear quartz was first made in quantity, and it uses the same burner idea as the Verneuil furnace for ruby (Synthetic Gems).

  1. The burner. A nozzle-mix oxy-hydrogen burner (Very-High-Temperature Furnaces), oxygen up the middle, hydrogen around it, roughly 2–2.5 volumes of hydrogen to 1 of oxygen. Fit a small hopper above it that taps grain into the oxygen stream, as in the Verneuil burner, or simply sprinkle grain from a spoon.
  2. Start a seed. Fuse two small crystals together in the flame, then hold the end of the joined piece — your seed rod — in the hottest part, just beyond the bright inner cone.
  3. Feed. Tap grain slowly into the flame. Each grain melts as it lands on the glowing tip and gives up its air. Turn the seed rod steadily, 1–2 turns a second, and draw it back as the clear lump grows, so the growing face stays at the same spot in the flame.
  4. Make rod. Once you have a clear lump 1–2 cm across, heat one end to a soft glow, touch on a second quartz rod, and pull apart steadily: you draw a quartz rod of 2–6 mm.
  5. Make tube by heating a clear lump, pressing a graphite rod into it, and working the glass round the graphite into a short thick tube, which is then reheated and drawn longer — or, more simply, build the tube up grain by grain on the end of a turning graphite rod.

Expect 20–50 g an hour from a small burner using roughly a cubic metre of hydrogen an hour. It is slow and costly, but it gives perfectly clear quartz for windows, lamp envelopes and UV work.

Method 2: Electric fusion — translucent tube

This is how most quartz tube for furnaces and chemistry was made in the early 1900s.

  1. The trough. A firebrick box 20–30 cm wide, 20 cm deep and 1–1.5 m long, with a copper clamp at each end.
  2. The rod. A smooth graphite rod 2–5 cm across, as long as the tube you want plus the clamps, turned true and polished (The Lathe).
  3. Bed it. Lay the rod in the trough clamped at both ends, and pack clean quartz sand all round it, 10 cm thick in every direction.
  4. Fire. Pass current through the rod from a low-voltage transformer: 10–30 volts at 500–2,000 amps, rising over 10–15 minutes. The rod glows white and a layer of sand round it fuses into a soft glass sleeve. 5–10 minutes at full heat gives a wall 3–8 mm thick.
  5. Pull the rod. Switch off, and while the sleeve is still red, draw the graphite rod out with a winch. The hot sleeve can be gripped at one end and blown (by compressed air through the rod hole) into a graphite or iron mould to make flasks, dishes and crucibles, or drawn out longer.
  6. Clean up. Break away the loose sand, and grind the rough outside smooth on a wet wheel if needed (Precision Grinding).

The result is white, translucent quartz tube with a glossy inside (from the smooth rod) and a sandy, satin outside.

In industry, clear tube is made continuously: crystal grain fed into a tungsten or molybdenum crucible heated electrically to above 2,000 °C in hydrogen, with the melt drawn out downward through a ring-shaped die round a central mandrel. That needs a mature high-temperature works.

Quartz crucibles

A quartz crucible holds molten silicon, salts and samples that would be ruined by clay or metal.

  1. Electric-fused: blow the soft sleeve from Method 2 into a graphite mould, or fuse it round a graphite former shaped like an upside-down cup, with the current passing through the former.
  2. Arc-fused: the industrial way for silicon-growing crucibles. Pour sand into a turning, water-cooled graphite mould so it lines the wall, then strike an arc between two graphite electrodes inside (The Electric Arc Furnace). The inside face melts to clear glass while the outside stays bubbly and white.
  3. Slip-cast: the easiest. Grind scrap fused quartz (never raw quartz) wet in a jar mill with flint pebbles (Ball Mills, Crushers and Grinders) for a day or two into a thick slip, cast it in plaster moulds exactly like pottery slip (Slip Casting, Jiggering and Ceramic Factories), dry it, and fire it to 1,150–1,250 °C for 2–4 hours. It sinters into a porous white crucible that keeps quartz's resistance to sudden heat. Do not fire hotter, or it turns to cristobalite and cracks.

Proportions: wall about one-twentieth of the diameter, never under 2 mm; a flat or gently rounded base; height no more than 1¼ times the width for melts.

Good versus bad. A good crucible rings when tapped, shows no white frost, and survives being heated in a flame and dropped into water (test a spare). A frosty patch is devitrification: discard it before it cracks in service.

Working quartz tube

Quartz is worked like borosilicate (Scientific Glassblowing and Glass-to-Metal Seals), with these differences:

  • The torch. A quartz-working torch burns hydrogen or natural gas with oxygen through 7–19 small jets (0.8–1 mm bore) that mix at the face, for a broad flame of about 2,000 °C on the work, with non-return valves and flashback bubblers on both lines.
  • No preheating: push quartz straight into the flame. But work fast: it stiffens within a second of leaving it. Keep it turning.
  • Graphite tools: paddles, rods and reamers; brass and iron stick and burn.
  • Clean: wipe with alcohol before heating, never touch the hot zone, and wash finished work in warm dilute hydrochloric acid and distilled water.
  • Flame deposit: the white haze beside a joint is fine silica; flash the flame over it to glaze it away.
  • Annealing: rarely needed; for precision work, half an hour at 1,100–1,200 °C, then cool slowly.
  • Joining to other glass needs a graded seal of about seven steps (Scientific Glassblowing and Glass-to-Metal Seals).
  • Eyes: shade 5–6 welding glass, not didymium.

The molybdenum foil seal

Double-ended linear lamp Pinch sealmolybdenum foil inside Coiled tungsten filament Support spiralkeeps it central exhaust tip Quartz envelope8–10 mm, krypton + bromine Capsule lamp filament both foils in one pinch pins The foil, end-on, magnified Knife edge Knife edge 0.02–0.03 mm thick in the middle quartz closes round it with no gap
Fig. 2 Inside a tungsten-halogen lamp. Top: a double-ended linear lamp. A long coiled tungsten filament is held on the axis by small tungsten spirals; at each end it is welded to a strip of molybdenum foil buried in a flattened pinch seal, which in turn is welded to the outer lead. The exhaust tip is in the middle. Below left: a capsule lamp with two pins. Below right: the foil seen edge-on, ground to knife edges so the quartz can close round it.

No wire expands as little as quartz, so no wire seals through it. The answer is to make the metal so thin that it bends instead of cracking the glass: a molybdenum foil seal.

  1. Foil: molybdenum (Molybdenum describes making it as powder, bar, wire and foil) 0.02–0.03 mm thick, 2–5 mm wide and 8–15 mm long.
  2. Knife edges. Etch the two long edges thin and sharp, for example electrolytically, with the foil as the positive electrode in a weak caustic soda solution, edges dipped in. With square edges the quartz cannot close round the foil and the seal cracks or leaks.
  3. Weld: spot-weld the tungsten filament lead to one end and a molybdenum outer lead wire (0.5–1 mm) to the other.
  4. Pinch: slide the assembly into the end of the quartz tube, flush the tube with nitrogen or argon so the molybdenum does not burn, heat the end to about 2,000 °C, and squeeze it flat with graphite-faced pinch jaws. The quartz flows round the foil and fuses to it.

Good versus bad. A good seal shows the foil as a bright, silvery strip with no bubbles along its edges. A dark or rainbow-coloured foil has oxidised and will leak. In use, the pinch must stay below about 350 °C: above that, air creeping along the outer lead burns the molybdenum and the lamp fails. That is why lamp fittings keep the pinch ends cool.

The halogen lamp

How it works

Filamentabout 3,000 °C Quartz wall 1. Tungstenmeets brominenear the wall:a gas forms Wall must beabove 250 °C tungsten boils off the filament 2. the gas drifts back and breaks apart in the heat bromine set free, goes round again 3. tungstenlands backon filament tungsten atombromine below 250 °C the tungsten stays stuck to the wall and blackens it
Fig. 3 The halogen cycle. Tungsten evaporates from the white-hot filament. Near the cooler wall, above about 250 °C, it combines with bromine (with a trace of oxygen) into a gas. The gas drifts back toward the filament, breaks apart in the heat, and leaves the tungsten on the filament again, freeing the bromine to repeat the trip. The wall stays clear.

In an ordinary bulb (The Light Bulb, Tungsten and Filament Wire), tungsten slowly boils off the filament and blackens the glass. Make the filament hotter for more light and it boils away faster.

Put a trace of bromine or iodine in the gas fill and something remarkable happens. Near the wall, tungsten atoms combine with the halogen into a gas. That gas wanders back to the filament, where the heat breaks it apart, leaving the tungsten on the filament and setting the halogen free to fetch more. This is the halogen cycle. It keeps the wall perfectly clear, but it works only if the wall is hotter than about 250 °C; below that, the tungsten compound stays on the glass.

A wall that hot means a small envelope close to the filament, which only quartz (or a special hard glass for small low-power lamps) can stand. And a small, strong quartz envelope can hold gas at several atmospheres, which slows the boiling-off further. So the filament can run hotter:

Ordinary lamp Halogen lamp
Filament about 2,700 °C about 2,900–3,000 °C
Light per watt 10–15 lumens 16–25 lumens
Life about 1,000 hours 2,000–4,000 hours
Light at end of life dimmer, bulb blackened almost as bright as new

The light is whiter, the lamp is small enough to put at the exact focus of a reflector or lens, and that is why halogen lamps lit car headlamps, film projectors, floodlights and theatres for fifty years.

Making one

A double-ended linear lamp (the floodlight type), for example 230 V, 300–500 W:

  1. Envelope: clear quartz tube 8–10 mm across, 1 mm wall, 80–120 mm long, with a short exhaust tube of 3 mm quartz fused into the middle of its side.
  2. Filament: a coiled tungsten filament on the axis (Tungsten and Filament Wire), with small tungsten wire spirals every 15–20 mm that touch the wall and hold it central.
  3. Seals: a molybdenum foil seal at each end, as above. Cap the ends later with ceramic caps over the outer leads.
  4. Pump and bake: pump through the exhaust tube to a good vacuum (The Vacuum Pump) while heating the envelope to 800–1,000 °C with a torch, and flash the filament gently to drive off gas.
  5. Fill: let in krypton or argon (Liquid Air, Nitrogen and the Noble Gases) containing a trace of bromine compound — a few tenths of a percent of hydrogen bromide or dibromomethane vapour (Bromine and Bromides) — or put in a tiny crystal of iodine (Iodine), a fraction of a milligram for a small lamp.
  6. Pressure: to get several atmospheres when cold, dip the lamp in liquid nitrogen (Cryogenics and Superconductors) while filling so the gas shrinks in, then tip off. Without liquid nitrogen, fill at a little under one atmosphere; the lamp works, with a shorter life.
  7. Tip off the exhaust tube with a sharp oxy-hydrogen flame, leaving a small pip.

A low-voltage capsule (12 V, 20–50 W) is a tube 9–12 mm across and 30–40 mm long, closed at one end, with a short compact filament across the middle and both leads through one pinch, as two pins.

Good versus bad. Run a new lamp 50 hours at full voltage. The wall should stay perfectly clear. Blackening means too little halogen, a leak, or a wall too cool (lamp too big for its wattage). Filament legs eaten thin near the seals mean too much halogen. White frost on the wall means fingerprints or salt devitrified it.

Using halogen lamps

  • Never touch the quartz; if you do, wipe it with alcohol before lighting.
  • Run at full voltage. Long dimming below about 80% cools the wall and the bulb blackens; a few minutes at full power clears it.
  • Keep the pinch cool in a ventilated fitting, and put a front glass before the lamp to stop ultraviolet and catch pieces if it bursts.

How to tell it worked

  • The water test. Heat a scrap of your quartz red-hot and drop it into cold water. Real fused quartz survives untouched; any glass shatters.
  • No sodium flare. In the torch flame, soft glass flares bright yellow. Clean quartz gives no yellow at all; a yellow flare means sodium contamination that will devitrify it.
  • Weight. Fused quartz weighs 2.20 g per cm³, lighter than window glass (2.5) and much lighter than crystal quartz (2.65): weigh a piece in air and in water.
  • Ultraviolet. Under a mercury lamp (Arc Lamps, Neon and Fluorescent Lights), a fluorescent mineral or paper behind quartz glows; behind ordinary glass it stays dark.
  • Strain. Between crossed polarisers (Polarised Light), well-made pieces show little colour.

Note Troubleshooting. Clear quartz full of bubbles → grain too fine or fed too fast; use clean 0.1–0.3 mm grain, feed slower. Brown or green tint → iron in the grain; wash longer in acid and crush between quartz, not iron. White frosty skin, then cracks → devitrification from fingerprints or salts, or held too long above 1,100 °C; clean better and work quickly. Electric-fused tube cracked along its length → rod pulled too late or unevenly; pull it while the sleeve is still red, straight and steady. Foil seal leaks or cracks → foil edges not sharp, or molybdenum oxidised during pinching; etch the edges and flush with nitrogen. Halogen lamp blackens quickly → too little halogen or a leak; too much halogen eats the filament legs instead.

Dangers

Danger Ultraviolet. A bare quartz lamp — halogen, mercury or arc — sends out ultraviolet that burns skin and eyes within minutes ("arc eye"). Always put ordinary glass in front of quartz lamps that light rooms, and never look at bare quartz UV lamps (Arc Lamps, Neon and Fluorescent Lights).

Danger Halogen lamps run hot and under pressure. The quartz reaches 250–900 °C and the gas inside is at several atmospheres when lit: a lamp can burst and throw hot quartz, and a floodlight can set curtains, paper or sawdust on fire. Use a guarded fitting with a front glass, keep it well away from anything that burns, and never touch a lit or recently lit lamp.

Danger Oxy-hydrogen flames and gases. Hydrogen explodes when mixed with air or oxygen; keep the gases separate until the torch tip, fit flashback arrestors, and light the hydrogen first (Hydrogen, Oxygen and Gases). Bromine compounds are poisonous and burn skin and lungs; methyl bromide in particular kills — handle halogen fills only in tiny sealed ampoules and in a fume hood (Bromine and Bromides). Iodine vapour irritates eyes and lungs (Iodine).

  • Heavy current in electric fusion burns deeply where a ring or tool closes the circuit: remove metal jewellery.
  • Silica dust from crushing and grinding quartz causes silicosis (Ball Mills, Crushers and Grinders): work wet, wear a respirator.

Going further

Synthetic fused silica, the purest of all, is made by burning silicon tetrachloride vapour (Pure Silicon) in an oxy-hydrogen flame; the fine silica smoke is fused into a glass that lets through ultraviolet down to about 0.16 µm. It is the starting material of optical fibre (Fibre Optics) and of the lenses that print microchips (Making Microchips). Quartz lamps with metal halides make the bright metal halide lamps of stadiums (Arc Lamps, Neon and Fluorescent Lights). Quartz tubes carry the furnaces of Pure Silicon and Integrated Circuits.

How it was first done

Marc Antoine Gaudin in France melted small pieces of rock crystal in an oxy-hydrogen flame in 1839 and drew them into threads. In 1887 Charles Vernon Boys in London drew extremely fine quartz fibres — by firing a molten-tipped arrow from a crossbow — for sensitive balances. Around 1899–1900, W. C. Heraeus in Hanau, Germany, with Richard Küch, began making clear fused quartz commercially with oxy-hydrogen flames, and Küch built the quartz mercury lamp a few years later. In 1903 the Thermal Syndicate in Wallsend, England, began making translucent quartz by fusing sand round electrically heated carbon rods. People had suggested putting chlorine in carbon lamps to stop blackening in the 1880s, but the practical tungsten-halogen lamp, with iodine in a quartz tube, was developed by Elmer Fridrich and Emmett Wiley at General Electric in the 1950s and went on sale in 1959; bromine fills followed in the 1960s.

Source: content/entries/earth/fused-quartz.md