Part 3 · Metals
Gold and Silver
Wash gold from river gravel with a pan and a sluice, take silver out of lead by cupellation, measure how much precious metal any ore holds with the fire assay and the touchstone, and refine both metals for money, mirrors, photography and electrical contacts.
- Difficulty
- ●●●●●
- Time
- Days to weeks of panning for a few grams of gold; an hour per cupellation once you have the cupels; a morning for a fire assay
- Steps from zero
- 13 prerequisites →
The full path from nothing — 13 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Pottery
- Hides and Leather
- Bellows
- Copper Smelting
- Lead
- Gold and Silver
Do them roughly in this order. See it on the tech tree →
Why it matters
Gold and silver are soft and too rare for tools. Their value is in four things no other metal does as well:
- They do not corrode. Gold never tarnishes at all; silver only darkens with sulfur. That makes them the metals for electrical contacts, fine wires and plating that must work for decades (see Electroplating).
- Silver is the best conductor of electricity and heat of all metals, and the most reflective. A thin film of silver on glass makes the best Mirrors and The Telescope mirrors.
- Silver compounds darken in light. That single property is the whole of Photography for its first 150 years.
- They hold value. Gold and silver are easy to test, easy to divide and impossible to counterfeit for anyone who knows the tests in this chapter. They make honest coinage and let strangers trade (see Money, Trade and Record-keeping).
Silver and gold also teach the most important skill in metallurgy: assaying — finding out exactly how much of a metal an ore contains, before you spend weeks smelting it.
How it works
Gold is found almost always as the native metal — tiny flakes, grains and occasional nuggets of real gold, usually alloyed with some silver. It is 19 times heavier than water — about seven times heavier than ordinary sand. In running water it sinks and stays while everything else washes away. Panning and sluicing use nothing else.
Silver is sometimes found native, but mostly it hides in other ores — above all in galena, lead ore (see Lead). When such galena is smelted, the silver goes into the lead. Cupellation then gets it out:
- Molten lead in a blast of air at about 900 °C burns to litharge (lead oxide), which melts at 888 °C.
- Molten litharge soaks into a porous dish made of bone ash, called a cupel, like water into a sponge, carrying copper and other base metals with it.
- Silver and gold do not burn. They are left behind on the cupel as a bright bead.
Molten lead also dissolves gold and silver from any crushed ore melted with it. So by smelting a weighed sample of ore with lead and cupelling the lead, you can collect and weigh every speck of precious metal in it. That is the fire assay, used for more than 3,000 years and still the most accurate test there is.
What you need
| Item | Notes |
|---|---|
| Gold pan | A shallow bowl 30–40 cm across with sloping sides: wood, metal or a smooth glazed pot. See Finding and Identifying Ores |
| Sluice box | Planks, about 2 m long; see below |
| Shovel, bucket, coarse sieve | A basket or sieve with 1–2 cm holes to screen out stones |
| Bone ash | For cupels: about 20 g per small cupel; burn bones yourself |
| Clay muffle and charcoal furnace | See below; or a forge with careful firing |
| Lead | Silver-free if possible, for assays. See Lead |
| Borax, or powdered glass and wood ash | Flux for melting gold and for assays |
| A fine balance | Able to show differences of a few milligrams. See Balances, Steelyards and Weighing Machines |
| Touchstone and touch needles | See below |
| Nitric acid (later) | For parting gold from silver. See Nitric Acid |
Where to find it
Gold. Gold forms in quartz veins in old, folded, hard rocks — slates, schists, greenstones and the edges of granite — and weathers out into streams. Look in rivers draining hilly country with white quartz veins. Within a stream, gold collects where the water slows and drops its heaviest load:
- the inside of bends, at the upstream end of gravel bars;
- behind large boulders and in natural riffles of ledges;
- in cracks and hollows of the bedrock under the gravel — dig down to it and scrape the cracks clean;
- on hard clay layers ("false bedrock") within the gravel;
- with the black sand — gold is always with it, though black sand is not always with gold.
Is it gold? Real gold in the pan is buttery yellow in sun and in shade, does not glitter or flash as you turn it, and does not move when you swirl the water. Press a flake with a knife point: gold flattens and dents, never breaks. Pyrite ("fool's gold") is paler, brassy, sparkles in flat faces, and crumbles to a black powder. Mica flakes glitter gold, but float and flutter in the water and fold like paper. Weathered brassy mica and chalcopyrite also crumble under a pin.
Silver. Native silver appears as wires, sheets and branching crusts in veins, usually tarnished black — scrape it and the cut is brilliant white. In dry country, the weathered tops of silver veins hold horn silver (silver chloride), a soft grey-green or brown waxy mineral that cuts with a knife like horn and darkens in sunlight. But for most people the realistic source is galena: test every galena you smelt.
Touchstone. You need a black, very fine-grained, slightly gritty stone that is harder than gold and does not react with acid: black chert or jasper ("lydite"), fine black slate, or dense black basalt. A pebble the size of your palm with one face ground flat and smooth is enough.
Borax. A white, crusty mineral found in the dry beds of desert salt lakes and around some hot springs; it tastes sweetish-alkaline and froths up when heated. If you have none, powdered clear glass mixed with a little Soda Ash and Baking Soda or wood ash does the same job.
Method 1: Panning and sluicing gold
Panning is described step by step in Finding and Identifying Ores. It is how you find gold — sampling one spot after another and counting the "colours" (specks) in each pan. To produce gold you need to wash much more gravel: a sluice.
Building a sluice
- Make a long open trough from three boards: a floor 25–30 cm wide and 1.5–2 m long, with sides 15 cm high. Seal the joints with clay or pitch.
- Lay a sheepskin with the wool on, a rough woollen blanket, or a mat of coarse sacking over the floor. Gold grains sink into the fibres and stay there. (The legend of the Golden Fleece probably comes from sheepskins used this way.)
- On top, fix riffles: wooden slats 2–3 cm high, across the box, every 10–15 cm, held by two long strips along the sides so the whole set can be lifted out.
- Set the sluice in a stream where the current is brisk, with the top end at a small dam or a channel that feeds water into it. Prop it so it slopes about 8–10 cm per metre of length.
Running it
- Adjust the water. It should run 5–10 cm deep and fast enough to roll small gravel along, with little whirlpools behind each riffle. If sand piles up and buries the riffles, steepen the slope or give more water; if the riffles are scoured bare, flatten it.
- Feed gravel slowly at the top — a shovelful every half minute — after screening out stones bigger than about 2 cm. Pay most attention to the bottom layer of gravel and the bedrock cracks: that is where the gold is.
- Clean up every few hours or at the end of the day. Stop the feed, let clear water run for a minute, then lift out the riffles and roll up the fleece carefully over a tub. Wash the fleece out in the tub.
- Pan the concentrate in the tub down to black sand and gold. Dry it. Draw a lodestone over it to remove magnetite. Blow gently across a dry pan of the last black sand: the light grains move and the gold stays. Pick out the gold with a wet fingertip or a feather. Heavy steel-grey grains that stay with the gold but are not gold may be crude Platinum and the Platinum Metals; keep them (see also Palladium, Rhodium and Iridium).
Gold from quartz veins must be crushed first — with hammerstones on a flat stone, then ground to flour on a quern or a mortar — and the powder panned. Old miners caught fine gold by rubbing the powder with mercury; read Mercury before ever doing this. It is one of the most poisonous jobs in the world, and careful panning recovers much of the gold without it.
Melting gold
Gold melts at 1,064 °C — the same heat as copper, a bright orange-yellow. Put the dry gold dust in a small fired-clay crucible with a pinch of borax (about a tenth of its weight), heat it in a charcoal fire under the bellows as in Copper Smelting, and when it spins into one bright ball, pour it into a warm, smoked stone ingot mould or let it cool in the crucible.
Method 2: Silver by cupellation
Making cupels
- Make bone ash. Burn clean animal bones in a hot fire for several hours, until they are white all the way through — black or grey means carbon is still in them. Crush them, grind them to flour, wash the powder in plenty of water (pour off the cloudy water and discard it), and dry it.
- Sieve the finest powder through tightly woven cloth.
- Moisten it with just enough water to hold together when squeezed — about 1 part water to 10 parts ash by weight. It should feel like damp sugar.
- Press it hard into a mould: a wooden or clay cup 3–4 cm across and 2 cm deep, with a rounded wooden stamp to make a smooth, shallow hollow about 1 cm deep in the top. Tap the finished cupel out.
- Dry the cupels for several days, then fire them gently. A cupel absorbs about its own weight of litharge: use a cupel at least as heavy as the lead you put in it.
The muffle furnace
The lead must have hot air flowing over it, not charcoal touching it — charcoal would turn the litharge straight back into lead. So the cupel sits inside a muffle: a small clay tunnel, about 20 cm long, 10 cm wide and 8 cm high, closed at the back, open at the front, made of the same clay as your crucibles and fired. Set the muffle in a charcoal fire (in a forge or a clay box furnace) so charcoal surrounds its sides, top and back, with the open mouth facing you. A hole or two in the back helps air flow through.
Step by step
- Heat the muffle until it glows bright cherry red to orange inside (about 900 °C), with the cupels inside to warm through for 10–15 minutes. A damp cupel will spit and crack.
- Charge. With long tongs, place a lump of the lead to be tested (5–30 g) in the hollow of each cupel. Close the mouth for a minute with a clay plug until the lead melts.
- The lead "opens". Open the mouth to let air in. The dull skin on the lead clears and the surface becomes bright and moving, with a glow of its own. Fumes rise gently from it. A dark ring of litharge spreads into the cupel.
- Hold the heat. You should see feathery crystals of litharge forming on the cupel's rim around the lead. If none form, it is too hot (and you are losing silver in the fumes); if the lead crusts over and stops moving ("freezes"), it is too cold — push in more charcoal and blow.
- The flash. As the last lead goes, the shrinking bead shows rainbow colours that ripple over its surface, then suddenly goes dull and then bright silver — the "blick" or flash. The lead is gone.
- Cool slowly. Draw the cupel to the front of the muffle for a minute before taking it out; a silver bead cooled too fast can spit (it gives off oxygen it absorbed while molten) and lose metal.
- Weigh the bead. Silver beads are white; a yellowish bead contains gold.
In bulk, the same thing is done on a larger, shallow hearth of bone ash or of wood ash packed into a clay or iron dish, 30–40 cm across. The bellows blow across the surface of the molten lead, and the litharge is pushed off over a notch in the rim as it forms, rather than all soaked up. Keep the litharge: smelted again with charcoal, it gives back the lead.
Method 3: The fire assay
This tells you how much silver and gold is in any ore or concentrate.
- Weigh 30 g of finely ground, dry ore.
- Mix it with about 60–90 g of litharge (made by burning lead in air, see Lead), 30 g of soda ash or wood ash, 10 g of borax or powdered glass, and 3 g of flour or fine charcoal powder. The flour turns some litharge back into lead; the rest acts as flux.
- Fuse it in a fired-clay crucible at bright orange-yellow (about 1,000 °C) for 30–45 minutes, until it bubbles quietly as a clear liquid.
- Pour it into a cone-shaped iron or stone mould. When cold, the lead lies as a button at the point, holding all the gold and silver. Hammer off the glassy slag.
- Cupel the button. Weigh the bead.
- Calculate. A 3 mg bead from 30 g of ore means 100 g per tonne (100 parts per million). That is rich ore.
Run every assay twice. If the two beads differ much, grind the ore finer and mix it better.
Method 4: Testing and refining
The touchstone
- Rub the gold on the flat face of the touchstone to leave a streak 2–3 cm long.
- Beside it, rub streaks from touch needles — strips of gold alloy of known fineness that you have made by weighing pure gold with silver or copper.
- Compare colours in good daylight. A trained eye can judge within a few percent.
- Acid test. Wet the streaks with a drop of nitric acid. Brass, copper and silver streaks fizz and vanish; gold stays. Low-gold streaks fade partly.
Gold fineness is given in karats: pure gold is 24 karat; 18 karat is 18/24 = 75% gold; 14 karat is 58%.
Parting gold from silver
Cupellation leaves gold and silver together. To separate them:
- Acid parting. If needed, melt in extra silver so the bead is about 3 parts silver to 1 part gold (with less silver the acid cannot reach it all). Hammer the bead into thin foil and warm it in nitric acid diluted with an equal volume of water. The silver dissolves; the gold is left as a brown, crumbly sponge that turns yellow when heated red. Pour off the silver solution and drop clean copper strips into it: the silver comes out as grey crystals you can melt into a bead. See Nitric Acid.
- Salt cementation (the ancient way, with no acid). Hammer the gold–silver alloy into thin foil. Pack it in a covered clay pot between layers of a mix of 2 parts powdered brick or fired clay to 1 part salt. Seal the lid with clay and keep it at a bright red heat (about 800 °C) for one to two days. The silver turns to silver chloride and soaks into the brick dust; the foil is left as nearly pure gold. Repeat for higher purity. Smelt the brick dust with lead and cupel it to get the silver back.
Hardening for use. Pure silver and gold are too soft for coins and cups. Sterling silver is 925 parts silver and 75 parts copper. Gold for coins and rings is alloyed with silver and copper to 22 or 18 karat.
How to tell it worked
- Gold stays bright when heated red and cooled; any tarnish means a base metal is present. It is soft and bends without cracking.
- Silver is bright white; heated in a flame and cooled, pure silver stays white; silver with copper goes dark.
- Weight: a gold piece is about twice as heavy as the same piece in silver or copper. Compare against a known sample of the same size, or weigh in water: gold of 18 karat or better weighs at least 15 times as much as the water it displaces.
Note Troubleshooting. Gold escapes the sluice → water too fast or too much; slope too steep; fleece missing. Test the tailings by panning them. Cupel cracked → it was damp or heated too quickly. Dry for longer; warm it in the muffle before adding lead. Lead freezes on the cupel → too cold. Push more charcoal round the muffle and blow; add a little more lead. Bead is grey and rough, or has a crust → copper or other metal remained. Cupel again with more lead. Bead vanished → it was too hot for too long, or there was no silver. Gold dust won't run together → it is too cool or dirty. More heat and a pinch more borax.
Dangers
Danger Lead fumes. Cupellation turns all the lead into fume and litharge. It is one of the most poisonous jobs in metalwork. Work only in the open air or under a tall chimney, upwind, and follow every rule in Lead. Keep children and pregnant women away.
Danger Nitric acid and its brown fumes. Parting gives off reddish-brown nitrogen dioxide, which damages the lungs. Symptoms can appear hours later and kill. Work outdoors, never breathe the fumes, and protect your eyes and skin. See Acids, Bases and Testing.
- Mercury. Never heat a gold–mercury amalgam in the open air. See Mercury.
- Cold water. Panning and sluicing all day in cold streams brings on hypothermia. Work in shifts, warm up often (see Surviving Cold and Heat).
- Mines and riverbanks collapse. See Mining and Tunnelling before digging into banks.
- People. Gold and silver attract theft and violence. Keep quiet about finds and store them securely.
What this unlocks
Silver dissolved in Nitric Acid gives silver nitrate, the starting point of Photography and of silvered glass Mirrors. Gold and silver films and contacts make reliable electrical connections; gold leaf hangs in the electroscope of Static Electricity and the Leyden Jar. Both metals coat others by Electroplating. Weighed and stamped, they become coins (Money, Trade and Record-keeping); worked fine, rings, chains and settings (Jewellery, Beads and Medals). The fire assay lets you judge any ore before you invest in smelting it.
How it was first done
Gold was probably the first metal people noticed: bright, unchanging nuggets in streams. The oldest large hoard of worked gold, more than 3,000 objects, was buried at Varna in Bulgaria between about 4,600 and 4,200 BC. Silver was being taken out of lead by cupellation by the 4th millennium BC in Anatolia and Mesopotamia. The silver mines of Laurion paid for the Athenian fleet in 483 BC.
The kingdom of Lydia, in western Turkey, struck the first coins around 600 BC from electrum, a natural gold–silver alloy. Under King Croesus, Lydians began minting separate gold and silver coins, and archaeologists have excavated the refinery at Sardis where gold was purified by salt cementation in the 6th century BC. The Greek writer Strabo described miners in the Caucasus catching gold on fleeces. Georgius Agricola's De re metallica (1556) illustrated sluices lined with cloth, cupellation hearths and assay furnaces in detail. The California gold rush of 1848–1855 made the sluice box famous. Justus von Liebig found how to deposit silver on glass in 1835, and Louis Daguerre made the first practical photographs on silvered plates in 1839.
Source: content/entries/metals/gold-and-silver.md