Part 8 · Chemistry
Water Softening and Ion Exchange
Certain grains, some natural (greensand, zeolites) and some made (gel zeolite, sulfonated coal, resin beads), grab the lime and magnesia out of hard water and give back harmless sodium. A barrel of them softens a household's water for weeks, and a few buckets of salt water restore them. Two columns in a row, one regenerated with acid and one with alkali, remove nearly every dissolved salt, giving water as pure as distilled for batteries, laboratories and boilers, and eventually the ultrapure water of chip factories.
- Difficulty
- ●●●●●
- Time
- A day to build a gravity softener from a barrel; a week to make a batch of gel zeolite; an hour to regenerate
- Steps from zero
- 32 prerequisites →
The full path from nothing — 32 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Sulfur
- Measurement from Scratch
- Writing and Numbers
- Hunting and Trapping
- Basic Woodworking
- Pottery
- The Kiln
- Charcoal
- Arithmetic and Fractions
- Hides and Leather
- Tiles and Clay Pipes
- Salt
- Lime
- Surveying and Levelling
- Fermentation
- Lye and Potash
- Glass
- Bellows
- Saltpeter
- Lead
- Copper Smelting
- Sulfuric Acid
- Pipes, Plumbing and Aqueducts
- The Battery
- Electrolysis
- Chlorine and Bleach
- Water Treatment for a Town
- Water Softening and Ion Exchange
Do them roughly in this order. See it on the tech tree →
Why it matters
Hard water, which has seeped through limestone, chalk or gypsum, carries dissolved calcium and magnesium. They cost a great deal:
- Soap curdles into scum, so a household in a chalk district can use two or three times the soap (Detergents and Wetting Agents, Soap).
- Boiled, the water leaves scale: stone on kettles, hot-water pipes and boiler plates. One millimetre of scale on a boiler plate makes the iron over the fire run 50–100 °C hotter, until it bulges and tears (Boilers and Pressure Vessels).
- Dyeing, laundry, tanning, brewing and paper-making all go wrong (Dyes and Mordants, Laundry and Bleaching Cloth, Hides and Leather, Paper).
Boiling, lime and washing soda soften water in batches, and leave some hardness behind. An ion exchanger does it continuously, at the tap, with nothing but salt, down to almost zero hardness.
The same principle goes further. A deioniser takes out not just the hardness but almost every dissolved salt, giving water as pure as distilled water, with no fuel. It is needed for battery topping-up, laboratory reagents and stains (Biological Stains, Identifying Substances), photography, high-pressure boilers (The Steam Turbine), and, polished to the extreme, the water that washes microchips (Making Microchips). Ion exchangers also refine sugar, recover metals from leach liquors (Leaching, Solvent Extraction and Electrowinning), and separate the Rare Earths, Cerium and Phosphors from one another (Separating the Rare Earths).
How it works
Salts dissolved in water split into charged particles called ions. Calcium and magnesium (the hardness) and sodium are positive ions; chloride, sulfate and bicarbonate are negative ions.
An ion exchanger is a solid grain that is a sponge full of fixed electric charges. Each fixed charge holds a loose ion of the opposite charge, which can swap with ions in the water flowing past.
Softening. The grains start loaded with sodium. Calcium and magnesium are held more strongly, so as hard water flows through, each calcium ion takes a place and releases two sodium ions. Out comes soft water: the same amount of dissolved salt, but sodium salts, which do not curdle soap or form scale.
Regeneration. When the grains are full of calcium, flood them with strong salt water, about 10 %. There is so much sodium that it pushes the calcium back off by sheer numbers, and the calcium runs to waste as calcium chloride. The grains are ready again. They last for years.
Deionising. Load one exchanger with hydrogen ions (by washing it with acid). It swaps every positive ion in the water for hydrogen, so the water comes out as a weak acid. Pass that through a second, anion exchanger loaded with hydroxide ions (by washing it with caustic soda). It swaps every negative ion for hydroxide. Hydrogen and hydroxide join to make water. What comes out is nearly pure.
Strength order. Exchangers prefer ions with more charge, and heavier ones: iron and aluminium over calcium, calcium over magnesium, magnesium over sodium, sodium over hydrogen. That is why softening works without effort, and why regeneration needs a flood.
Measuring hardness. Hardness is counted as milligrams of chalk per litre. Rainwater has under 20; water from limestone wells, 200–400. The soap test in Detergents and Wetting Agents measures it without instruments.
What you need
| Item | Notes | See |
|---|---|---|
| Exchanger | Greensand, natural zeolite, gel zeolite, sulfonated coal or resin beads: below | |
| Tank | Barrel, drum or tank: wood, stoneware, concrete or steel lined with pitch or enamel. Not bare iron for a deioniser | Barrels and Cooperage, Tins, Cans, Drums and Tanks |
| Gravel, washed and graded | 2 cm down to 3 mm, for the underdrain | |
| Pipes and taps | Four taps or a multiway valve | Pipes, Plumbing and Aqueducts |
| Salt | For regeneration: 3–4 g per gram of hardness removed | Salt |
| Acid and caustic soda | For a deioniser | Hydrochloric Acid, Sulfuric Acid, Lye and Potash |
| Soap solution, silver nitrate | For tests | Detergents and Wetting Agents, Silver Nitrate and Silver Salts |
Where to find it
- Greensand is a sand or soft sandstone coloured dark olive or bottle green by grains of glauconite, a mica-like mineral of iron and potassium that formed on old sea floors. Look in marine sandstones and marls: the Lower and Upper Greensand of southern England, the greensand marls of New Jersey, belts in Belgium, northern France, Russia and Australia. The grains are rounded, 0.1–1 mm, soft enough to crush with a knife blade, and stain the fingers faintly green. Farmers have long dug it as a slow potash fertiliser (Compost and Manure).
- Natural zeolites are white, cream or pinkish minerals full of tiny channels. They occur as beds in altered volcanic ash (soft, light, pale tuff, often in old lake beds), and as crystals filling the gas holes of basalt lavas: radiating needles, white cubes or glassy blocks. Their name means "boiling stone": heat a chip in a flame and it froths and swells as water bubbles out of the channels. They are lighter than ordinary rocks and scratch easily with a knife. Clinoptilolite and chabazite are the most useful kinds.
- Coal, kaolin, sand and soda ash for synthetic exchangers: Coal and Coke, Finding and Preparing Clay, Soda Ash and Baking Soda, Water Glass (Sodium Silicate).
- Clay and soil exchange ions too. That is how soil holds fertiliser (Understanding Soil), but clay packs into mud and cannot be used in a column.
The exchangers
| Exchanger | Capacity, g chalk per litre of bed | Regenerate with | Strengths and weaknesses |
|---|---|---|---|
| Greensand, natural | about 6–7 | Salt | Free if you have it; low capacity; tolerates nothing acid |
| Natural zeolite (clinoptilolite) | low for hardness | Salt | Best for removing ammonia from fish ponds and wastewater (Fish Ponds) |
| Gel zeolite (synthetic) | about 20–25 | Salt | High capacity; dissolves slowly in acid or very soft water |
| Sulfonated coal | about 10–15 | Salt, or acid | Survives acid, so can be used in a deioniser |
| Polystyrene resin beads | 40–60 in use | Salt, or acid | Modern standard; needs a petrochemical works |
| Anion resin | 20–40 | Caustic soda | Needed for deionising |
Capacities vary with the water and the salt dose; treat these as starting figures and measure your own.
Greensand and natural zeolite
- Wash the greensand in a trough of running water, stirring, until the water runs clear. Clay and silt float away.
- Sieve it, keeping grains between about 0.3 and 1 mm.
- Harden it (optional but it lasts much longer): soak it in thin Water Glass (Sodium Silicate) solution, drain, and dry it at about 100 °C, then rinse.
- Prepare it by running a 10 % salt solution through it once, then rinse.
Crush zeolite rock to 0.5–2 mm and use it the same way. Test a handful in a jar with hard water first: shake, settle, and soap-test the water before and after.
Gel zeolite (synthetic)
Made from Water Glass (Sodium Silicate) and alum, the gel zeolite gave the first commercial softeners. This outline needs trials to get right:
- Dilute water glass with about twice its volume of water. Dissolve alum in water separately (Alum and Alumina).
- Stir the alum solution into the water glass slowly until the whole mass sets to a jelly. Keep the mixture alkaline (litmus stays blue); if it turns acid you get a useless powder.
- Let it stand overnight. Cut the jelly into lumps and dry them slowly, below about 100 °C, to hard glassy pieces.
- Drop the dry pieces into water. They crack into grains. Sieve to 0.5–2 mm, wash out the fines, and rinse with salt water.
A second route, fusing kaolin, sand and soda ash together in a crucible and crushing the cold melt, gives a harder but lower-capacity material (The Kiln).
Sulfonated coal
Crushed bituminous coal (Coal and Coke), sieved to 0.5–1.5 mm, is stirred into strong sulfuric acid (about three parts acid to one of coal) and kept hot, near 100–150 °C, for several hours. The acid attaches acid groups to the coal. Cool, pour slowly into a large volume of water (never water into acid), wash until the washings are no longer sour, and rinse with salt water. Because it survives acid, sulfonated coal can be regenerated with acid into the hydrogen form: the first half of a deioniser.
Ion-exchange resin
Modern exchangers are plastic beads 0.3–1.2 mm across: polystyrene cross-linked with a little divinylbenzene so it swells without dissolving, then soaked in hot strong sulfuric acid, which adds acid groups to every ring. They are amber, glassy and perfectly round, and they last ten years or more (Petrochemicals and Modern Plastics). The beads are made by stirring the liquid monomers into hot water so they break into droplets, which harden as they polymerise.
An earlier, more achievable route: a phenol–formaldehyde resin made from phenol that has first been heated with sulfuric acid, so it already carries acid groups (Early Plastics, Methanol and Formaldehyde). Cure it hard, crush and sieve it. A resin of formaldehyde with an amine gives a weak anion exchanger.
Anion resins that can take out every negative ion, even silica and carbon dioxide, need strong amines and a carcinogenic intermediate. They are for a works with proper ventilation and training.
A good resin: round, unbroken beads that sink in water; no fines; capacity holding steady over many cycles. Cracked, cloudy or fine beads mean it has been dried out, frozen, or attacked by chlorine.
Method 1: A water softener
Size it. A barrel 40 cm across and 1 m tall holds about 60 litres of exchanger in a 50 cm deep bed. With greensand at 6.5 g per litre, that is about 400 g of hardness between regenerations: 1,300 litres of water at 300 mg per litre. The same barrel filled with resin softens about 10,000 litres. Work it out for your water and your household's use.
Build it:
- Underdrain. Lay a pipe across the bottom of the barrel, drilled with rows of 3 mm holes, capped at one end, the other end out through the wall to the soft water tap. Wrap it in a single layer of coarse cloth, or cover the holes with saw cuts narrower than your grains.
- Gravel. Cover the pipe with 15 cm of graded gravel: coarse (2 cm) at the bottom, then medium (8 mm), then fine (3 mm) on top, each layer levelled.
- Exchanger bed 50 cm deep on the gravel.
- Freeboard. Leave at least 25–30 cm of empty space above the bed. In backwash, the bed lifts and expands by a third to a half; without room it washes away.
- Spreader. The inlet at the top ends in a perforated pipe or a tin plate pierced with holes, so the water does not dig a crater in the bed.
- Taps: inlet (hard water in at top), soft water out (bottom pipe), backwash in (hard water into the bottom pipe), waste (from the top, above the bed, to the drain). The brine tank feeds in at the top.
- Brine tank set higher than the softener: a barrel of salt with water over it, which stays at about 26 % saturated brine. Draw from it through a tap.
Soften: open inlet and soft-water taps. Flow gently: about 5 m per hour downwards for greensand, which is 600 litres an hour through a 40 cm barrel. Faster lets hardness slip through.
Regenerate when the soap test shows the water turning hard:
- Backwash for 10 minutes: hard water upward through the bottom pipe, out through the waste tap. Watch the bed lift and swirl; stop if grains start to wash out. This loosens the packed bed and carries away dirt and fines.
- Brine: let the bed settle and drain the water down to just above the bed. Run in 10 % brine, about 3–4 g of salt per gram of hardness to be removed: for the barrel above, 1.4 kg of salt in 14 litres. Let it soak down slowly over 20–30 minutes.
- Rinse downward with hard water to waste until the water no longer tastes salty, and a drop of silver nitrate in a test tube of it gives no more than a faint cloud. This takes about three bed-volumes.
- Back into service.
Industrial version: closed steel pressure vessels in pairs, one softening while the other regenerates, switched by a multiport valve, often by a clockwork or water-meter timer (Clockwork, Music Boxes and Counting Machines).
Good and bad softeners. A good one gives a constant soap-test reading of 1–2 mL (as soft as rainwater) to the end of its run, with no salty taste. Hardness leaking early means channelling (the water finding a path down one side), a bed packed with dirt, or too little brine. Grains in the soft water mean a broken underdrain.
Method 2: A deioniser column
Two-bed deioniser. Two glass or lined columns in a row. For a laboratory, each is a glass tube 4–5 cm across and 60 cm tall, with a cotton or glass-wool plug and a rubber tube and clip at the bottom (Laboratory Glassware).
- Cation column: fill with sulfonated coal or strong cation resin. Regenerate with 5–7 % hydrochloric acid (about two bed-volumes, slowly), or 2 % sulfuric acid. Stronger sulfuric acid deposits gypsum inside the bed. Rinse with distilled or deionised water until the effluent is only slightly acid.
- Anion column: fill with anion resin. Regenerate with 4 % caustic soda, rinse until the rinse is barely alkaline.
- Run the water through the cation column first, then the anion column, slowly: about one bed-volume every 5–10 minutes.
Mixed bed. Cation and anion resins mixed in one column give much purer water, because each ion meets both kinds of grain many times. To regenerate, backwash: the lighter anion resin floats to the top and the cation resin sinks. Drain and regenerate each layer separately, through taps at top, middle and bottom. Then remix the two by bubbling air up through the bed. A two-bed then mixed-bed train gives laboratory-grade water.
Capacity: a 1-litre bed of resin deionises roughly 100–200 litres of ordinary tap water, much more of rainwater. Pre-soften or pre-distil very hard water.
Chlorine destroys resins. Pass chlorinated town water through a bed of Activated Charcoal first.
Conductivity cell
Pure water hardly conducts electricity; dissolved salts make it conduct. A conductivity cell measures purity directly.
- Make it: two parallel plates 1 cm square, 1 cm apart, of platinum, or nickel, stainless steel or carbon, fixed in a glass tube with open ends so water fills the gap. Lead wires out through the top sealed in glass or wax.
- Measure the resistance between the plates with alternating current; direct current coats the plates with gas and gives false readings. An old-style bridge with a buzzer for current and an earphone to listen for the silent balance point works (Measuring Electricity, Electronic Test Equipment).
- Read it: for a cell of these dimensions, conductivity in microsiemens per centimetre (µS/cm) is 1,000,000 ÷ resistance in ohms.
| Water | Conductivity (µS/cm) | Resistance in this cell |
|---|---|---|
| Sea water | about 50,000 | 20 Ω |
| Hard well water | 500–1,000 | 1–2 kΩ |
| Rainwater | 10–50 | 20–100 kΩ |
| Good distilled water | 1–5 | 200 kΩ–1 MΩ |
| Two-bed deionised | 1–10 | 100 kΩ–1 MΩ |
| Mixed-bed deionised | 0.1–1 | 1–10 MΩ |
| Theoretical pure water | 0.055 | 18 MΩ |
Conductivity rises about 2 % per °C, so measure at room temperature and note it. Regenerate when the deioniser's output rises above your limit, say 10 µS/cm for battery water.
Without instruments: a drop of silver nitrate in deionised water stays perfectly clear; evaporate 100 mL to dryness in a clean glass dish and there is no ring of residue; it gives a rich lather with the first drop of soap solution.
Ultrapure water, in outline
A microchip factory needs water so pure that a speck of salt per thousand million parts spoils a chip (Making Microchips). The train: filter; Activated Charcoal; reverse osmosis (pumping water at high pressure through a membrane that lets water through but not salts, removing 95–99 % of everything; see Membranes, Reverse Osmosis and Desalination); two-bed deionisers; ultraviolet lamps to break down traces of organic matter; a final polishing mixed bed; and a 0.2 µm filter. The water reaches 18.2 MΩ·cm, the limit set by water's own splitting into ions, and runs in a constant loop through plastic pipes, never metal, never standing still.
How to tell it worked
- Softener: the soap test on output water reads 1–2 mL, like rainwater; kettles stop furring; soap lathers at once.
- Deioniser: conductivity steady and low; silver nitrate test clear; no residue on evaporation.
- Regeneration: the first run after regeneration is as long as the one before. Capacity falling steadily over months means fouling by iron, oil or organic matter, or chlorine damage.
Note Troubleshooting. Hard water slips through early → too fast a flow, channelling, or not enough brine; backwash well and give a full salt dose. Softened water tastes salty → rinse longer. Grains in the outlet → broken underdrain cloth or slots. Brown or orange bed → iron in the water; see below. Bed packs solid → dirt and fines; backwash more often, and filter muddy water first (Water Treatment for a Town). Deionised water acid → the anion column is exhausted or too small; regenerate it. Gel zeolite turning to mush → acid or very soft water dissolving it; use sulfonated coal or resin instead.
Iron and manganese. Well water with iron turns laundry and baths orange. Manganese greensand is greensand soaked in Potassium Permanganate solution until it is coated with dark brown manganese oxide. Water passing through has its dissolved iron and manganese oxidised and trapped, to be washed out by backwash. Regenerate it with permanganate.
Dangers
Warning Softened water carries extra sodium: about 46 mg per litre for every 100 mg of hardness removed. That matters for people on salt-restricted diets, people with heart or kidney failure, and infant feeds. Leave one unsoftened tap for drinking and cooking, and do not water plants with softened water.
Danger Acid and caustic for regenerating a deioniser burn skin and eyes. Mix and pour them with goggles and gloves, always adding acid or caustic to water. Hot strong sulfuric acid for making sulfonated coal or resin gives off choking fumes; work outdoors.
- Deionised water is not sterile. Idle beds grow bacteria. Never use it for injections or wounds; that needs freshly distilled, sterilised water (Intravenous Fluids, Sterilising Instruments and Dressings).
- Deionised water eats copper and iron pipes, because it is hungry for ions. Store and pipe it in glass, plastic or tin-lined vessels.
- Brine waste spoils soil and drinking water. Drain it to a river or sea, not into a field or near a well.
What this unlocks
Soft feedwater for Boilers and Pressure Vessels and The Steam Turbine plant; battery water for The Rechargeable Battery banks; pure water for The Medical Laboratory, Photography and Electroplating; softened water for Laundry and Bleaching Cloth and dye houses; the separation of Rare Earths, Cerium and Phosphors (Separating the Rare Earths) and recovery of uranium (Nuclear Energy (Overview)); and the ultrapure water of Making Microchips.
How it was first done
In 1850 the English agricultural chemists Harry Thompson and John Thomas Way showed that soil swaps the ammonia of manure for its own calcium, and Way found the clay minerals responsible. In 1858 Heinrich Eichhorn showed that natural zeolites exchange ions reversibly. The German chemist Robert Gans patented synthetic aluminosilicate softeners from about 1905, sold as Permutit, and processed greensand softeners spread through America in the 1910s and 1920s. Sulfonated coal followed in the 1930s. In 1935 Basil Adams and Eric Holmes at the government Chemical Research Laboratory at Teddington, England, made the first synthetic resin exchangers from phenol and amine resins, which made deionising possible. In 1944 Gaetano D'Alelio at General Electric patented the sulfonated polystyrene bead used ever since. In the 1940s, in work that grew out of the Manhattan Project, Frank Spedding's group at Ames, Iowa, used long ion-exchange columns to separate the rare earths from one another by the kilogram.
Source: content/entries/chemistry/ion-exchange.md