◆ Rebuild

Part 10 · Machines

Bearings and Lubrication

Every turning shaft rests in a bearing, and every bearing lives or dies by its grease. How to make wooden, bronze and babbitt-lined bearings, how to choose and make lubricants, and what it takes to make ball and roller bearings.

Difficulty
●●●●●
Time
An hour for a greased wooden bearing; a day to cast and bore a bronze bush; a day to pour and scrape a babbitt bearing
Steps from zero
15 prerequisites →

You need first

The LatheBronze

This unlocks

Ball Mills, Crushers and GrindersThe Potter's WheelMaking Ball and Roller BearingsCentrifugal Pumps and FansLubricants and GreasesPowder MetallurgyThe Motor VehicleThe Bicycle
The full path from nothing — 15 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Fire
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. The Wheel and Axle
  12. Bellows
  13. The Lathe
  14. Copper Smelting
  15. Bronze
  16. Bearings and Lubrication

Do them roughly in this order. See it on the tech tree →

Why it matters

A machine is mostly a collection of things that turn or slide against other things. Wherever a shaft turns, it rests in a bearing — and every bearing is a place where friction eats power, heat builds up, and metal or wood wears away. A cart axle without grease squeals, smokes and can catch fire; a mill shaft without grease grinds itself oval in a week; a steam engine with a dry bearing seizes in minutes. Old engineers said a machine is only as good as its bearings, and lubrication is everything.

Good bearings let a The Waterwheel or The Windmill pass more of its power to the stones; let Gears mesh truly because their shafts stay put; let a The Lathe turn round work; and let the The Steam Engine, Railways and generators run fast for years. This chapter goes from a greased hardwood block to the cast babbitt bearing of the industrial age, and explains honestly what ball bearings need.

How it works

Friction

When two surfaces slide, their tiny bumps catch and tear. The force needed to keep them sliding, divided by the load pressing them together, is the friction coefficient. Typical values:

Surfaces Friction coefficient Meaning
Dry wood on dry wood 0.3–0.5 A third to half the load is needed just to slide it
Greased wood on wood, or iron on wood 0.05–0.15
Greased iron on bronze, slow 0.05–0.1
Shaft running fast in a full film of oil 0.002–0.01 The metal surfaces do not touch at all
Ball or roller bearing 0.001–0.003

All of the lost work becomes heat — which is why a dry bearing gets hot, and a hot bearing is the first warning of trouble.

How oil carries the load

A lubricant does two jobs. At slow speeds and heavy loads, a layer of fat or oil clinging to each surface keeps the bumps from tearing each other: boundary lubrication. Friction is reduced, but there is still wear.

At speed, something remarkable happens. A shaft always sits slightly off-centre in its hole, so the gap between them is wedge-shaped. As the shaft turns, it drags oil round with it and squeezes it into the narrow part of the wedge. The oil cannot escape fast enough, its pressure rises, and the shaft lifts off the bearing and floats on a film of oil thinner than a hair. With a full film there is almost no wear at all; a well-oiled engine bearing can run for decades. This needs three things: enough speed, a smooth round shaft in a smooth round hole with a small, even gap, and a steady supply of oil.

Split pillow block (end view) The oil wedge Oil cupwool wick feeds drops Babbittlining3–6 mm Shaft Shimspaper Cap Base, bolted downremove a shim to take up wear lift Wide gapoil dragged in Narrow wedgepressure lifts shaft Turning shaftfloats on oil, never touches gap hugely exaggerated
Fig. 1 A plain bearing. Left: the split pillow block, with a babbitt lining, an oil hole, a groove to spread the oil, and thin shims between the halves to take up wear. Right: why oil carries the load — the turning shaft drags oil into the narrowing gap, building pressure that lifts the shaft off the metal.

Choosing a bearing

  • Slow, heavy, dirty (cart axles, waterwheel shafts, millstone spindles, windmill posts): a greased plain bearing of hardwood, stone, bronze or iron.
  • Fast and loaded (line shafts, engines, lathes): a plain bearing of bronze or babbitt, kept full of oil.
  • Load pushing along the shaft (an upright mill shaft carrying gears and a millstone; a propeller; a drill): a thrust bearing, often a footstep — the rounded end of the shaft sitting in a cup of hard material.
  • Very fast, light, or needing the lowest friction (bicycle wheels, small motors, precision spindles): ball or roller bearings, if you can make them hard and accurate enough.
Split wooden block Footstep (thrust) Bronze bush Ball bearing Greasepocket, pegged Splitplane facesto tighten Hornbeamor lignumvitae Uprightshaft Roundediron tip Cupsteel or stone beam Oil hole Groovestops shortof the ends Bronzepressed intohousing Outerrace Balls Inner race Shaft hard, round, all the same size
Fig. 2 Four kinds of bearing. A split hardwood block with a grease pocket for slow shafts; a footstep, where the rounded end of an upright shaft turns in a hard cup and carries its weight; a bronze bush with an oil hole and groove; and a ball bearing, where hardened balls roll between two hardened rings.

What you need

Item Use Notes
Hardwood blocks Wooden bearings Hornbeam, lignum vitae, oak, apple, boxwood; boiled in fat
Bronze Bushes and bearing shells About 88% copper, 10% tin, 2% lead — see Bronze
Babbitt (white metal) Bearing linings About 89% tin, 7–8% antimony, 3–4% copper, or a lead-based mix (below)
Tallow, lard Grease Rendered animal fat
Slaked lime Thickens grease See Lime
Non-drying oil Oiling fast bearings Rapeseed, olive, neatsfoot, castor; later mineral oil (Petroleum and Refining)
Graphite powder Added to grease for heavy, slow, hot jobs
Soot (lamp black) or red ochre in oil "Marking" for scraping
Tools The Lathe, scraper (an old file ground to a flat or three-cornered tip), ladle, clay, files

Where to find it

  • Bearing woods. The best is lignum vitae — a very heavy, olive-brown tropical wood (Caribbean and northern South America) so full of natural resin that it lubricates itself, even under water. It sinks in water. Outside the tropics, use hornbeam, apple, holly, boxwood or the heart of old oak; boiling these for an hour in tallow fills their pores and doubles their life.
  • Tin, antimony and copper come from their ores: tin from cassiterite (heavy brown-black pebbles in stream gravels, see Tin and Pewter), antimony from stibnite (lead-grey needle crystals that melt in a candle flame, see Finding and Identifying Ores), copper from Copper Smelting ores.
  • Fats. Suet — the hard fat round the kidneys of cattle and sheep — gives the firmest tallow. Pigs give soft lard. Render either by heating gently in water and skimming.
  • Oils come from pressing seeds and fruit (Oils and Pressing). Avoid linseed (flax) and walnut oil: they are drying oils that turn to a sticky varnish in air and glue a bearing solid. Test any oil: smear a drop on glass or a smooth stone and leave it a week. If it is still slippery, it is a good bearing oil; if it is tacky or skinned over, reject it.
  • Graphite — soft, black, greasy mineral that marks paper — occurs in old metamorphic rocks (see Pencils and Chalk).

Method 1: Wooden and stone bearings

For slow shafts — carts, waterwheels, mill gearing, windmill posts, pump handles.

  1. Make the block. Take a block of hornbeam, lignum vitae or oak at least 1.5 times as long as the shaft is thick, and as thick again around the hole. A 10 cm shaft wants a block 15 cm long with at least 5 cm of wood all round.
  2. Split it. Saw the block in half along the line of the shaft so the top can be lifted off. Bore or carve the hole with the halves held together, then separate them. A split bearing lets you lift the shaft out and lets you tighten the bearing when it wears, by planing a little off the faces where the halves meet.
  3. Set the grain right. Put the end grain of the wood against the shaft if you can (the block cut across the trunk), or at least have the grain running across the shaft, not along it. End grain wears far more slowly.
  4. Fit loosely. Leave 0.5–1 mm of play for a wooden bearing. Wood swells when damp; a tight wooden bearing will bind and burn.
  5. Cut a grease pocket. Carve a hollow 2 cm across in the top half, with a hole through to the shaft, and keep it packed with tallow. Plug it with a wooden peg to keep out dirt.
  6. For thrust, set the end of an upright shaft in a footstep: a cup cut in a block of hard stone (flint, quartzite) or, better, a hardened steel or bronze cup set in a wooden beam. Round the shaft end to a blunt cone and fit it with an iron or hardened steel tip if you can. Keep the cup full of grease.

Method 2: A bronze bush

A bush (bushing) is a tube of bearing metal pressed into a frame. Bronze is strong, wears slowly, does not seize easily on iron or steel, and can be cast and bored on a lathe.

  1. Cast a thick tube of bearing bronze (see Metal Casting): outside 1.5 times the shaft size, length 1–2 times the shaft size, with the hole cast undersize.
  2. Bore the hole on the The Lathe to fit the shaft. For an iron shaft running in bronze, the gap (the running clearance) should be about one thousandth of the shaft diameter, plus a little: about 0.03–0.05 mm on a 25 mm shaft, 0.1 mm on a 75 mm shaft. Without a fine gauge, aim for a fit where the oiled shaft slides in with a gentle push, turns freely by hand, and you cannot feel any shake when you try to rock it.
  3. Turn the outside so it is a tight push or hammer fit into its housing. It must never turn in the housing.
  4. Drill an oil hole through the top, and with a narrow chisel or a round file cut a shallow oil groove along the inside, from the hole to within 5 mm of each end — never all the way out, or the oil runs straight out of the ends.

Method 3: A babbitt-lined bearing

Babbitt (white metal) is a soft alloy, mainly tin or lead, holding hard little crystals of antimony and copper compounds. The soft metal lets dirt bury itself harmlessly and lets the bearing shape itself to the shaft; the hard crystals carry the load. If oil fails, babbitt melts before the steel shaft is ruined — the bearing is the part you replace. It melts at only about 240–370 °C, so it can be poured into a bearing shell in a forge fire, with no lathe needed to bore it.

Kind Mix by weight Use
Tin babbitt (best) Tin 89, antimony 7–8, copper 3–4 Engines, fast shafts
Lead babbitt (cheaper) Lead 80, antimony 15, tin 5 Slower, lighter work, line shafting
  1. Make the alloy. Melt the copper first with a little of the tin (copper melts at 1,085 °C, but dissolves in hot tin far below that). Add the antimony, then the rest of the tin. Stir with a green stick, skim the dross and cast into small bars.
  2. Prepare the shell. The shell is the cast-iron or bronze housing, split in two halves (a pillow block). Its inside should be rough or have dovetail grooves or a few 6 mm holes drilled part-way into it, so the babbitt locks in. Clean it to bare metal.
  3. Set up the mould. Lay the shaft (or a dummy bar of the same size) in the lower half. Smoke it in a candle or oily-rag flame until it is black with soot, so the metal will not stick. Centre it with packing so the gap all round is equal — 3–6 mm of babbitt for small bearings, up to 10 mm for big ones. Dam the ends with stiff clay rolled into sausages, leaving a pouring hole and a vent at the top.
  4. Preheat the shell until a drop of water sizzles hard on it but does not dance about — about 120–200 °C. A cold shell freezes the babbitt before it fills.
  5. Heat the babbitt in an iron ladle until a dry pine splinter dipped in it browns and smokes in two or three seconds but does not burst into flame — about 420–450 °C for tin babbitt, but only about 340–370 °C for lead babbitt, which gives off more lead fume the hotter it gets. Hotter burns out the tin; colder pours lumpy.
  6. Pour in one steady stream until metal shows at the vent. Let it cool for 15 minutes.
  7. Do the top half the same way, with thin cardboard or a few layers of paper soaked in oil (the shims) laid between the halves so you can later remove shims to take up wear.
  8. Trim and scrape (see below). Cut the oil hole and oil grooves.

Scraping to a fit

No pour or boring is perfectly true. Scraping makes the shaft bear evenly over the whole surface.

  1. Smear the shaft thinly with soot or red ochre mixed with oil (the marking).
  2. Put the shaft in the bearing, clamp the cap lightly and turn it a few times.
  3. Take it out. The marking has rubbed off onto the high spots of the bearing.
  4. Shave each marked spot lightly with the scraper.
  5. Repeat until the marks are small, even spots all over the bearing — 70–80% of the surface. Twenty or thirty rounds are normal. A good fit shows as many small shiny islands, not a few big ones.

Lubricants

The main kinds, in short; Lubricants and Greases gives full recipes, oil cups and grease cups.

Lubricant How to make it Best for
Tallow Render hard fat, strain through cloth, wash in hot water Slow wooden bearings, gears, cart axles
Axle grease Tallow and pine tar (Tar, Pitch and Glue) half and half Outdoor, wet, dirty bearings: carts, waterwheels
Lime grease ("cup grease") Warm about 8 parts tallow; stir in 1 part slaked lime made into milk with water; keep stirring at a gentle heat until it thickens to a stiff soap, then thin with oil. Do not cook it bone-dry or it separates (full method in Lubricants and Greases) Stays put better than tallow and water does not wash it out; softens at 80–100 °C; good for slow metal bearings
Graphite grease Stir 1 part fine graphite into 4 parts tallow Very heavy, slow loads; hot bearings
Bearing oil A non-drying oil (above), left to settle and decanted clean Fast metal bearings, engines, line shafts
  • Keep it clean. Grit in grease turns it into grinding paste. Store lubricants covered; wipe a bearing before opening it.
  • Fat goes sour. Old fat turns acid and eats metal. Wash tallow in hot water (or water with a little wood ash) when rendering, and use it fresh.
  • Feed oil steadily. An oil cup above the bearing with a twist of wool yarn hanging down as a wick siphons oil drop by drop. A ring oiler — a loose brass ring hanging on the shaft and dipping into an oil bath below — carries oil up as the shaft turns.

Ball and roller bearings

Rolling instead of sliding cuts friction almost to nothing. But a ball bearing only works if the balls are all the same size (within a few thousandths of a millimetre), round, very hard, and run in hardened tracks (races). Soft balls flatten in hours; uneven balls carry the load on one or two and crack. This needs hardened bearing steel, Precision Grinding and precise measurement — an industrial skill, not a first step. Making Ball and Roller Bearings teaches it once you have them.

The achievable route is rollers for slow, heavy loads:

  • A roller ring for a turntable or windmill cap. Set 10–20 short hardwood or iron rollers, 5–8 cm thick, in a wooden ring (the cage) that keeps them evenly spaced, running between two flat iron or hardwood tracks. Windmill caps, cranes and turntables have turned on such rings for centuries.
  • Steel balls, when you get there, are forged roughly round from bar, then ground between two grooved plates turning against each other with oil and fine abrasive (Abrasives and Grinding Stones), measured, sorted into batches by size, and hardened.

How to tell it worked

  • The hand test. After an hour of running, put your palm on the bearing. If you can hold it there comfortably, it is fine (under about 50 °C). If you must pull away after a few seconds, it is running hot — find out why. If spit sizzles on it, stop at once: it is over 100 °C and about to seize or burn.
  • The smell. Hot tallow smells of frying; hot oil smells sharp; burning wood smells like a fire. Any of these means stop.
  • The sound. A good plain bearing is silent. Knocking means too much play; squealing means it is dry.
  • The shake test. With the machine stopped, lift the shaft with a bar near the bearing. Visible movement means it is worn and the shims should come out or the bearing should be re-lined.

Note Troubleshooting. Bearing runs hot → too tight, out of line with the other bearings, dry, or the oil grooves are blocked. Loosen the cap a little and check the oil reaches the shaft. Bearing hot only at one end → the shaft is not in line. Shim the housing until a string stretched along the shaft passes through the centre of every bearing. Grease thrown out and lost → too thin or too hot; use lime grease or add graphite. Babbitt cracks or comes loose → shell not clean, not keyed, or too cold when poured; re-pour. Babbitt full of holes → the shell was damp or the metal too cold. Dry and preheat it. Wooden bearing swelled and seized → too tight; allow 1 mm play and keep it greased so water cannot soak in.

Dangers

Danger Molten metal and water explode. Babbitt poured into a damp shell, a wet ladle or onto clay that has not dried throws molten metal out violently. Dry every tool and mould by the fire first. Wear thick leather and protect your eyes. Lead babbitt gives off poisonous lead fumes and dust — work in the open air, upwind, never eat or smoke while handling it, and wash your hands (see Lead). Antimony fumes (white smoke) are also poisonous.

  • Fire. A dry wooden bearing under load can char and set fire to a mill. Many water and windmills burned this way. Grease daily and feel the bearings on every round.
  • Seizing. A seized bearing on a powered shaft can twist off the shaft or throw belts and gears. Shut down at the first sign of heat.
  • Oily rags soaked in drying oils can heat themselves and catch fire. Spread them out to dry or keep them in a closed metal or clay pot.

Going further

How it was first done

Greasing wooden axles goes back as far as wheels; tallow and pitch have been found on ancient cart axles. Footstep bearings of stone carried the upright shafts of potter's wheels and mills from the earliest days. The Roman Nemi ships, built for the emperor Caligula about AD 40 and raised from Lake Nemi in the 1930s, carried rotating platforms that turned on bronze balls and wooden rollers held in cages — very early rolling bearings.

Leonardo da Vinci sketched ball and roller bearings around 1500. The Welsh inventor Philip Vaughan patented a ball bearing for carriage axles in 1794, but balls good enough for real service came only with the bicycle boom of the 1870s–1880s; in 1883 Friedrich Fischer in Schweinfurt, Germany, built a machine to grind steel balls accurately. Isaac Babbitt, a Boston metalworker, patented his white-metal bearing in 1839. In 1883 Beauchamp Tower found by experiment that a well-oiled shaft floats on pressurised oil, and in 1886 Osborne Reynolds explained why — the theory behind every oiled bearing since.