◆ Rebuild

Part 6 · Building

Window Glass

How to turn molten glass into flat panes — by casting, by spinning a crown, or by blowing and flattening a cylinder — and how to cut them, set them in wooden frames with linseed putty or join them with lead, plus oiled paper, horn and mica windows for before you have glass.

Difficulty
●●●●●
Time
Weeks to build the furnaces; a day per batch of panes once you can blow glass; an hour to glaze a window
Steps from zero
7 prerequisites →

You need first

Glass

This unlocks

Cold Frames, Cloches and Greenhouses
The full path from nothing — 7 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Pottery
  5. Lime
  6. Lye and Potash
  7. Glass
  8. Window Glass

Do them roughly in this order. See it on the tech tree →

Why it matters

Before glass, a window was a hole: you could have light or warmth, but not both. In winter people lived in smoky half-darkness, with shutters closed against the cold. Glass windows let daylight into rooms while keeping out wind, rain and insects — which means reading and close work indoors in winter, warmer houses, healthier air in workshops, sickrooms that can be kept clean (Sanitation and Germs), and greenhouses that grow food out of season (Cold Frames, Cloches and Greenhouses, Solar Heat).

Flat glass is also the starting point for mirrors (Mirrors), glass plates for Photography, and the glazed fronts of instruments. This chapter assumes you can melt and blow glass (Glass); here we make it flat, cut it and set it in a window. It also gives you translucent windows of paper, horn and mica that you can make long before you have a glass furnace.

How it works

Glass is soft and workable between about 700 and 1,100 °C (see the colour table in Glass). To make a flat sheet you must spread the soft glass thin and even without touching it more than you must, because every tool mark and every cool spot shows as a ripple. There are three old ways:

  1. Casting — pour the melt onto a flat bed and spread it. Simple, but the glass is thick, uneven and only translucent: one face is smooth, the other picks up the texture of the bed.
  2. Crown — blow a bubble, open it, and spin it so fast that it flares into a flat disc. The fire-polished surface is brilliantly clear, but the panes are small and there is a thick lump (the bullseye) in the middle.
  3. Cylinder — blow a long cylinder, cut it open along its length, and let it sag flat in a hot kiln. Bigger panes, slightly less brilliant.

All flat glass must then be annealed — cooled slowly from about 520 °C — or it will crack later (Glass).

The batch. For windows you want the clearest glass you can make. Use the whitest sand or crushed white quartz you can find, washed; avoid sand stained yellow or red, which is iron, and which turns glass green. Soda-lime glass (Glass, Soda Ash and Baking Soda) is clearest and easiest. Forest glass made from raw wood ash works but is green or brown; it still lets in plenty of light.

What you need

Item Notes
A glass furnace, crucibles and a melt Glass. For windows you need more glass per day: several kilograms
A glory hole A small, very hot reheating furnace with a round opening 20–30 cm across
Blowpipes and punties Iron tubes 1.2–1.5 m and solid iron rods (Blacksmithing)
A flattening kiln For the cylinder method: a chamber that can hold 600–700 °C, with a smooth flat stone or fired-clay floor
An annealing oven Glass
Cutting tools A rod of iron to heat red-hot; a hardened Steel point or wheel, a diamond, or a sharp flake of flint or quartz; a straight-edge
A grozing iron A flat iron bar with slots of different widths cut in its end, for nibbling glass edges
Linseed oil and whiting For putty: Oils and Pressing; whiting is chalk ground and washed to a fine white powder
Lead For leaded lights (Lead), and tin for solder (Tin and Pewter)

Method 1: Cast panes

The Romans glazed their bath-houses and villas this way. It is the best first method because it needs no blowing skill.

  1. Prepare a bed. A smooth, flat slab of stone or fired clay, dusted with fine dry sand or wood ash so the glass does not stick, with a frame of iron or stone bars 4–6 mm high laid on it to set the size and thickness. Preheat it near the furnace until it is too hot to touch (200–300 °C) — glass poured on a cold bed cracks.
  2. Pour. Ladle or tip a puddle of molten glass, bright orange, into the frame.
  3. Spread it quickly into the corners with iron tongs or a hooked rod, and press it flat with a smooth, wetted wooden block or an iron roller laid across the bars.
  4. Anneal at once. As soon as it has stiffened (dull red, after a minute or so), slide it into the annealing oven on a flat iron peel and anneal it as in Glass.
  5. Trim the edges with a grozing iron.

Cast panes are 3–6 mm thick, with one smooth face and one matt face. They are translucent rather than clear — you see light and shapes, not a view — but they keep out the weather perfectly. Grinding and polishing both faces with sand and water on a flat stone (Abrasives and Grinding Stones) makes them clear, but this is days of work for each pane.

Method 2: Crown glass

Crown glass needs a good glassblower (Glass) and a strong, steady assistant.

1. Blow a globeflatten its end 2. Move to a puntythe pipe end opens 3. Reheat and spinfaster and faster 4. It flashes flata disc, seen edge-on Bullseyethick lump where the punty wasPanescut from the clear part around it5. CUT
Fig. 1 Making crown glass. Blow a bubble and flatten its end; move it to a punty; reheat it and spin it fast until it flashes open into a flat disc; anneal it; then cut panes from around the bullseye.
  1. Gather a large lump of glass on the blowpipe — 1–3 kg for a disc 40–70 cm across. Build it up with several gathers, marvering between each.
  2. Blow a globe about 25–30 cm across. Flatten the end opposite the pipe on the marver, making the globe like a squat onion.
  3. Transfer to a punty. Attach a hot punty with a blob of glass to the centre of the flattened end. Crack the blowpipe off, leaving a round hole where it was.
  4. Reheat the piece in the glory hole until it is soft and bright orange all over, turning the punty steadily so it does not droop.
  5. Spin. Take it out and spin the punty fast between your hands or on a rest, faster and faster. The hole widens, the glass rushes outward, and suddenly — in a second or two — it flashes open into a flat disc. Keep spinning until it stiffens, with the disc held upright.
  6. Anneal. Break the punty off and stand the disc on edge in the annealing oven, supported so it cannot warp.
  7. Cut. Cut rectangular panes from around the bullseye (below). The bullseye itself, thick and lumpy, was traditionally sold cheap for back windows and stables.

A disc 60 cm across gives about four panes of roughly 20 × 25 cm. Crown glass is thin (2–3 mm), fire-polished and very clear, with faint curved ripples.

Method 3: Cylinder glass

1. Blow and swinginto a long cylinder 2. Cut off both endsthen split it lengthwise 3. Soften at 600–700 °Cit unrolls on the kiln floor 4. Smooth it flatwith a wet wooden block,then anneal
Fig. 2 Making cylinder glass. Blow and swing a long bubble into a cylinder; cut off both ends; split it along its length; then let it soften and unroll flat in the flattening kiln, smoothing it with a wooden block, before annealing.
  1. Gather and blow a large, thick bubble, as for crown glass.
  2. Swing it. Standing over a pit or on a platform, swing the blowpipe like a pendulum while blowing, reheating often. Gravity stretches the bubble into a long, even cylinder. Aim for 30–60 cm long and 15–25 cm across at first; skilled blowers made cylinders well over a metre long.
  3. Open the end. Heat the far end in the glory hole and blow, so the soft end bursts or can be cut open; or wrap a thread of hot glass around it, let it cool a moment, and touch it with a wet stick — it cracks off clean.
  4. Cut off the pipe end the same way. You now have an open tube, called a muff.
  5. Split it along its length: draw a red-hot iron rod slowly along the line (see "Cutting glass" below), or score it and tap.
  6. Flatten. Lay the split cylinder, crack upward, on the smooth, sanded floor of the flattening kiln at 600–700 °C (a dull-to-cherry red glow). In a few minutes it softens and slowly unrolls. Help it with a wet wooden block on an iron rod, pressing it flat and smooth.
  7. Anneal the sheet immediately.

Cylinder panes are larger than crown panes and have no bullseye, but the face that lay on the kiln floor picks up some texture. Polish it with a fine wet sand and a felt pad if you need it clearer.

Cutting glass

Glass breaks along a scratch or a crack, not where you want it, unless you guide it.

  1. The hot-iron method (the medieval way, needing no diamond). Make a small nick at the edge with a file, a hard stone or a sharp flint. Heat the tip of an iron rod red-hot and hold it just ahead of the nick: a crack starts. Draw the iron slowly along the line you want, 2–3 mm ahead of the crack; the crack follows the heat. A wet finger touched behind the iron sharpens it. With practice you can follow curves.
  2. Scoring. A diamond, a hardened steel point or (best) a small wheel of very hard steel, drawn firmly once along a straight-edge, leaves a fine, even scratch. Hold the glass on each side of the score and bend it sharply away from the scratch; it snaps clean. Score only once; never go over a line twice.
  3. Grozing. Nibble away unwanted edges and refine curves with the slots of the grozing iron, a little at a time.
  4. Edges. Rub sharp edges smooth on a flat sandstone with water.

Glazing with putty

A SASH BAR, CUT ACROSSLEAD CAME, CUT ACROSS Front puttybevelled at 45°GlassBed putty2–3 mmPinpresses the glass inSash barrebates primedwith linseed oilRebateabout 1 × 1 cmoutsideinside Flangeabout 6 mm wideHeartGlassCementoil, whiting, soot panel seenfrom insideSaddle bar
Fig. 3 Glazing a wooden sash. The glass sits on a thin bed of putty in a rebate cut in the frame, held by small pins, and is sealed with a bevel of front putty. A leaded light joins small pieces with H-shaped lead strips.

Make the putty. Grind chalk to powder, mix it with plenty of water, let the grit settle for a minute, pour off the milky water and let the fine whiting settle from it; dry it. Mix whiting into raw linseed oil, kneading hard, until you have a stiff dough that does not stick to your hands: roughly 1 part oil to 6–7 parts whiting by weight. Keep it wrapped or under oil; it hardens slowly in air.

Glaze:

  1. The window frame (the sash) needs a rebate — a step cut in the inner edge of each bar, about 1 cm deep and 1 cm wide — for the glass to sit in (Basic Woodworking).
  2. Prime the rebate with a coat of linseed oil and let it soak in; bare wood sucks the oil out of putty and it crumbles.
  3. Bed. Press a thin layer of putty (2–3 mm) into the rebate.
  4. Set the glass, cut 2–3 mm smaller than the opening all round. Press it into the bed by its edges until putty squeezes out behind.
  5. Pin it with small headless nails or hardwood pins pushed into the frame against the glass, every 20–25 cm.
  6. Front putty. Roll putty into a thin sausage, press it along the edge of the glass, and smooth it into a bevel at 45° with a knife held at an angle, so rain runs off. Its top edge should be just below the line of the frame on the inside, so it is invisible from the room.
  7. Trim the bed putty squeezed out behind.
  8. Let it skin for 1–2 weeks, then paint over it with linseed oil paint (Pigments, Paints and Varnish), lapping the paint 1–2 mm onto the glass to seal the joint.

Leaded lights

Leaded windows join many small pieces — scraps, cast pieces or uneven crown glass — into one large window. They are also how coloured glass windows are made.

  1. Make the came. Cast lead (Lead, Metal Casting) into a two-part mould carved with H-shaped grooves, giving strips 40–60 cm long with a cross-section like a capital H lying on its side: two flanges about 6 mm wide joined by a thin heart, leaving a channel each side for the glass. Draw them straight and smooth them with a wooden tool.
  2. Draw the window full size on a board (the cartoon). Cut each piece of glass to the pattern, allowing for the heart of the lead.
  3. Assemble on the board, starting from one corner against two nailed battens. Fit each piece into the came, tap it home with a wooden stick, and hold it with nails driven into the board alongside.
  4. Solder each joint where cames meet, on both sides, with tin-lead solder and a soldering iron heated in the fire, using tallow as flux (Soldering and Brazing).
  5. Cement it: brush a thin paste of linseed oil, whiting and soot under the flanges on both sides, then dust with whiting, clean off, and press the flanges down. This makes it waterproof and stiff.
  6. Support it. Lead is soft. Fix iron saddle bars across the inside of the window every 30–40 cm, and tie the panel to them with copper wire soldered to the leads. Keep each panel under about half a square metre.

Before glass: other windows

  • Oiled paper or cloth. Stretch thin Paper or fine linen on a frame and rub it with linseed oil or melted fat; it turns translucent and sheds rain. Renew it every year. Japanese houses still use paper screens indoors.
  • Horn. Soak cattle horn for weeks, or boil it until soft, slit it open and flatten it under weight between warm boards. Scrape and press it into sheets about 1 mm thick (Horn and Bone Working). Horn lets through a warm yellow light and does not break. Small panes of horn glazed lanterns ("lanthorns") for centuries.
  • Mica. Some rocks contain books of clear, flexible mica that split into thin sheets. Russian builders glazed windows with mica, and it was sold abroad as "Muscovy glass". It also makes excellent stove windows, because it does not crack in the heat (Chimneys, Stoves and Heating).
  • Membranes. Scraped and stretched animal bladder, parchment or gut — Arctic peoples made windows of seal gut. Translucent and light, though they let little heat stay in.

Keeping the heat in

A single pane loses heat many times faster than a thick wall. In cold climates:

  • Shutters inside or out, closed at night, save most of the loss. Heavy curtains help.
  • Double windows. A second sash fitted inside the first for the winter, with a still air gap of 5–15 cm between them, more than halves the loss. Russian and Scandinavian houses have done this for centuries.
  • Seal the frame to the wall with lime mortar or oakum (tarred fibre). See Insulation and Keeping Buildings Warm or Cool for the rest of the house.

How to tell it worked

  • Panes lie flat on a table without rocking, and you can see through crown or cylinder panes with only gentle waviness.
  • A pane survives being stood in the cold air and then held near a fire for a minute without cracking — proof it is well annealed.
  • Glazed windows do not rattle, and no daylight shows around the edges. In driving rain, no water comes through.
  • After a month the putty has a firm skin and has not cracked away from the glass.

Note Troubleshooting. Panes crack days later for no reason → poor annealing. Anneal longer and cool more slowly (Glass). A crown will not flash open → not hot enough, or not spun fast enough. Reheat to bright orange and spin harder. Cylinder sheets stay wavy → the flattening kiln is too cool; work at cherry red and press it flat. The crack wanders off the line when cutting → the hot iron is too far ahead or too cold; keep it close and red-hot. Putty crumbles and falls out → rebate not primed, or too little oil in the putty. Leaded panel bulges → too few saddle bars, or panel too big. Glass is green → iron in the sand; find whiter sand. Green glass still makes a good window.

Dangers

Danger Broken glass cuts deep. Carry sheets upright, by their edges, with leather gloves or pads, and never across your body. A falling pane can cut an artery. Sweep up every fragment. If someone is badly cut, press hard on the wound and see Wound Care and Antiseptics.

Danger Lead is a poison that builds up in the body and damages the brain, especially in children. Wash your hands after handling lead, never eat or drink while working with it, melt it outdoors upwind, and keep children away from lead work and lead dust (Lead).

  • Molten and hot glass and the glory hole cause severe burns; a spinning crown can throw drops of hot glass. Keep everyone back while flashing, and wear thick clothing of wool or leather, never loose plant fibre that catches fire (Glass).
  • Furnace glare. Staring into a white-hot furnace for years damages the eyes; glance, don't stare.
  • Falls when fitting windows high up — use a scaffold or a tied ladder (Scaffolding and Ladders).

What this unlocks

Clear flat glass leads to mirrors (Mirrors), glass plates for Photography, greenhouses and cold frames (Cold Frames, Cloches and Greenhouses), lanterns (Lamps and Candles), and the windows of instruments like the The Barometer and The Thermometer. Ground and polished, it gives Optical Glass and Achromatic Lenses for Lenses and Spectacles.

How it was first done

The Romans were the first to glaze windows widely, in the first century AD, using cast panes; examples survive in the baths of Pompeii and Herculaneum. The cylinder method was described around 1120 by the German monk Theophilus in his craft handbook, On Diverse Arts, and medieval glaziers set its colourful pieces in lead to make the windows of the great cathedrals. Crown glass was made in Normandy by the 1300s and in England from the late 1600s, and gave the small-paned windows of Georgian houses. Polished cast plate glass for large mirrors and windows was developed in France in 1688. In the 1830s British makers improved the cylinder process so much that the Crystal Palace in London (1851) could be glazed with nearly 300,000 identical panes. In 1959 the British firm Pilkington introduced float glass, made by floating molten glass on a bath of molten tin — the method used for almost all window glass today.

Source: content/entries/building/window-glass.md