◆ Rebuild

Part 3 · Metals

Tin and Pewter

Smelt tin by the kilogram from heavy black stream pebbles, refine it, alloy it into lead-free pewter for plates, cups and spoons that never rust, and coat iron with it to make tinplate for cans and kitchenware.

Difficulty
●●●●●
Time
Days of panning for each kilogram of ore; a day per smelt; an afternoon to cast pewter; a day to tin a batch of iron sheets
Steps from zero
9 prerequisites →

You need first

Finding and Identifying OresCharcoalBellows

This unlocks

Canning and BottlingCutlery and TablewareSoldering and BrazingTins, Cans, Drums and Tanks
The full path from nothing — 9 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Identifying Ores
  5. Hunting and Trapping
  6. Basic Woodworking
  7. Charcoal
  8. Hides and Leather
  9. Bellows
  10. Tin and Pewter

Do them roughly in this order. See it on the tech tree →

Why it matters

Tin is the metal that makes other metals better. One part of tin in ten turns soft copper into Bronze. Tin with lead (or with a little copper) makes solder, the glue of metalwork, without which there are no wire joints, no sealed cans and no electrical circuits (see Soldering and Brazing). A thin skin of tin on iron sheet makes tinplate, which does not rust and can be cut, folded and soldered into cans, lanterns, funnels, cups and kitchen pots. A thin skin of tin inside a copper pot keeps acid food from dissolving the copper.

On its own, tin becomes pewter: tin hardened with a few percent of other metals. Pewter melts on a kitchen fire, casts beautifully in simple moulds, never rusts, and makes plates, cups, jugs, spoons, candlesticks and buttons. For centuries it was the tableware of ordinary households.

Tin also brings food preservation into the modern age: the sealed tin can is the heart of Canning and Bottling.

How it works

Tin's only important ore is cassiterite, tin oxide (SnO₂). Like other oxide ores, it is smelted by heating it with charcoal: carbon monoxide gas from the burning charcoal takes the oxygen away and leaves metallic tin. Three facts shape the whole process:

  1. Tin oxide holds its oxygen tightly. It needs more heat and a more strongly smothered fire than copper ore — a yellow heat, about 1,100–1,200 °C, with the ore buried in charcoal.
  2. Tin melts at only 232 °C. As soon as it is free, it is liquid. It trickles down through the charcoal and collects at the bottom, where it can be tapped out while the furnace is still running.
  3. Tin oxide also dissolves in slag. If there is much sand (silica) in the charge, tin is lost into a glassy slag. So the ore must be very clean — washed until it is nearly pure black grains — and the slag must be smelted again.

Because tin melts so low, it is also easy to refine: the impurities (mostly iron) melt much higher, so gentle heat lets pure tin run away from them.

What you need

Item Amount Notes
Cassiterite concentrate 5–20 kg per furnace smelt; 200 g for a crucible test Washed, nearly pure black grains. See Finding and Identifying Ores
Charcoal About 2 kg per kg of concentrate, plus 10 kg for preheating Pieces 1–3 cm. See Charcoal
Clay, sand, grog 50–80 kg For a small shaft furnace. See Finding and Preparing Clay
Bellows and 2 tuyeres See Bellows
A sloping clay or stone refining hearth 1 About 50 × 30 cm. See below
Copper 2–3% of the tin For pewter. See Copper Smelting
Antimony 5–7% of the tin (optional) For Britannia-type pewter. From stibnite, see Antimony and Bismuth
Moulds Soapstone, brass or bronze, plaster or sand. See Metal Casting
Iron sheet, tallow, a large iron pot For tinplate See below

Where to find it

Cassiterite comes from granite country: the coarse, speckled, pink-white-and-black rock. It forms in quartz veins at the edges of granite, and as the granite weathers, the heavy, almost indestructible cassiterite washes into streams. Stream tin — rounded brown-black pebbles and grains in gravel — is how most ancient tin was found, and it is still the easiest source.

Cassiterite is astonishingly heavy (about 7 times water, more than two and a half times ordinary stone), glassy to greasy brown or black, too hard to scratch with steel, and gives a pale streak — that last test tells it from look-alikes. Pan the streams as described in Finding and Identifying Ores; cassiterite stays in the pan with the black sand and any gold. Follow the tin upstream to find the richest gravels.

Cleaning the concentrate. Your goal is a concentrate that is at least two-thirds cassiterite.

  • Pan or sluice it repeatedly (a sluice is described in Gold and Silver).
  • Dry it and draw a lodestone over it to pull out the magnetite (see Magnets).
  • Pick out light-coloured grains (quartz, feldspar) by hand on a flat board.
  • Wolframite, a tungsten ore, often occurs with tin and looks similar. It is a little heavier, often splits into flat plates, and has a dark brown to black streak. Pick it out; save it — Tungsten and Filament Wire is valuable later for Alloy and Stainless Steels.

A good concentrate is so heavy that a cupful weighs nearly four times as much as a cupful of water.

Warning In some tin districts the ore comes with arsenopyrite — silvery, brassy-white crystals that smell of garlic when struck. When roasted or smelted it gives off deadly white arsenic smoke. If your concentrate smells of garlic on a hot stone, roast it first in the open air, upwind, as described in Finding and Identifying Ores, and keep everyone away from the smoke.

Method 1: A test smelt in a crucible

Before you build a furnace, prove your ore. The crucible method is given in full in Bronze: mix one volume of concentrate with one volume of powdered charcoal, bury the crucible deep in charcoal under the blast, hold it at a yellow heat for an hour, then break out the beads of tin. If you get silvery beads that melt easily on a cooking fire, you have tin ore.

Method 2: The tin shaft furnace

To make tin by the kilogram, use a small shaft furnace like the one in Iron (the Bloomery), but shorter, with a channel that lets the tin run out as it forms. Cornish tinners used furnaces of this kind, called blowing houses, for centuries.

Clay shaft60–80 cm high,20–25 cm inside Tuyere10–12 cm above thefloor, sloping down from the bellows Blue-tinged flamea smothered, reducing fire Charge1 kg charcoal, then0.5–1 kg clean concentrate Yellow heat1,100–1,200 °C at the tuyere Tin trickles downit is liquid above 232 °C Tap holefloor slopes toward it Basintin under charcoal dust
Fig. 1 A small tin shaft furnace in cross-section. Tin trickles down through the charcoal, runs out through the tap hole and collects in a basin outside, under a layer of charcoal dust.

Building it

Part Size
Inside diameter 20–25 cm
Height of shaft 60–80 cm
Wall 8–10 cm of clay mixed with equal parts sand or grog, plus chopped straw
Tuyere 10–12 cm above the floor, sloping down about 15°
Floor Sloping 1 in 10 toward a tap hole 2–3 cm wide at floor level
Basin A clay-lined hollow outside the tap hole, 15 cm across and 6–8 cm deep
  1. Build on dry, level ground. Make a floor of packed clay sloping gently toward the front.
  2. Build the shaft in rings of clay, as in Iron (the Bloomery), setting the tuyere at the back and leaving the tap hole at the front at floor level.
  3. Dig and line the basin in front of the tap hole, so tin running out of the hole falls into it.
  4. Dry the furnace slowly for several days, then with a gentle wood fire inside for a day.

Smelting

  1. Preheat. Fill the shaft with charcoal, light it, and blow gently for an hour until the walls glow orange inside. Keep the tap hole open but loosely plugged with charcoal.
  2. Charge. When the level sinks 10–15 cm, add 1 kg of charcoal and then 0.5 kg of concentrate, spread evenly. After the first few charges, if the furnace is running hot, increase the ore to 0.75–1 kg per kg of charcoal.
  3. Blow steadily. Keep a strong, even blast. You want yellow heat in front of the tuyere and a lazy blue-tinged flame at the top — the sign of a smothered, reducing fire.
  4. Watch the tap hole. Within the first hour, bright tin begins to dribble out into the basin. Keep the basin covered with a layer of charcoal dust so the tin does not burn in the air.
  5. Clear the slag. If the tap hole chokes with sticky slag, open it with a green stick or an iron rod. Rake out slag on to dry sand and keep it — it is still rich in tin.
  6. Finish. After the last ore, blow for another 20–30 minutes with charcoal only.
  7. Ladle out the tin from the basin with a preheated iron or clay ladle and pour it into ingot moulds of stone or sand.
  8. Resmelt the slag. Crush the cooled slag, pan out any beads of tin, and feed the crushed slag back into the next smelt as part of the ore. Old tinners smelted their slags two or three times.

A clean concentrate that is 70% cassiterite contains about 55% tin. A first furnace may recover half of that; a practised crew, with slag resmelting, much more.

Refining tin

Raw tin from the furnace contains iron, which makes it hard, grey and crumbly, and sometimes copper or arsenic. Two simple steps clean it.

  1. Liquation. Build a small sloping hearth of clay or flat stones, about 50 × 30 cm, tilted 1 in 6, with a small fire or charcoal bed underneath, and a clay-lined pot at the low end. Lay the raw tin ingots on the high end. Heat the hearth gently — below any red glow, about 250–350 °C; a dry pine shaving laid on the hearth should brown slowly but not flame. Pure tin melts and runs down into the pot. Iron-tin alloy, which melts much higher, stays behind as a crusty spongy lump called hardhead (save it and resmelt it).
  2. Poling. Heat the liquated tin in an iron or clay pot to about 300–350 °C. Push a thick stick of green wood down to the bottom of the pot and hold it there. It boils off steam and gas, which stir the tin violently and bring dross up to the surface. Skim the dross off with a preheated iron skimmer. Repeat until the surface stays bright for several seconds after skimming.
Raw tin ingotslaid on the high end Hardheadiron-rich lump stays behind slope about 1 in 6 Pure tin runs offdown the hearth Clay potkept warm Gentle heatno red glow; 250–350 °C ladle out, pourinto ingot moulds
Fig. 2 Refining tin by liquation. Gentle heat melts the tin out of the raw ingots; it runs down the sloping hearth into the pot, leaving the iron-rich hardhead behind.

Method 3: Pewter

Pure tin is soft and weak: a pure-tin spoon bends in porridge. A few percent of other metals make it much harder while keeping it easy to cast and shine.

Alloy Recipe by weight Character
Fine pewter (simplest) 97 parts tin, 3 parts copper Bright, strong enough for plates, cups and spoons
Britannia metal 92 parts tin, 6 parts antimony, 2 parts copper Harder and stiffer; can be hammered and spun into thin vessels (see Metal Spinning and Raising)
Old "trifle" and "lay" pewter Tin with 5–25% lead Do not make it. Lead leaches into food and drink. See Lead

Never put lead in pewter for food or drink. Old pewter often contains lead; if you salvage old pewter of unknown origin, use it for buttons, candlesticks and fittings, not tableware.

Alloying

Copper melts at 1,085 °C, far hotter than tin. Do not try to melt copper in your tin pot. Instead, make a hardener first:

  1. In a crucible in the copper furnace (see Copper Smelting), melt 1 part copper. When it is liquid, add 1 part tin and stir with a green stick. Pour it out in thin strips on to dry sand. This 50/50 alloy is brittle and silvery-grey and melts at a dull red heat.
  2. Melt your tin in an iron or clay pot over a wood fire. Add the hardener (6 parts of hardener to every 94 parts of tin gives 97% tin, 3% copper) and raise the heat to a dull red just visible in shade until the hardener has dissolved. Stir well.
  3. Let it cool back to casting heat before pouring.

For Britannia metal, add antimony in the same way, wrapped in a twist of tin foil and stirred under, with the melt covered by a layer of charcoal.

Casting pewter

Pewter is cast at about 280–330 °C — hot enough that a slip of paper dipped in it turns brown in a couple of seconds but does not flame. Too hot and the metal oxidises and the moulds suffer; too cool and it freezes before it fills.

  • Moulds. Soapstone is ideal. Pewterers also used reusable moulds of brass or bronze, cast from a pattern of the object (see Metal Casting), and these last for generations. Sand and plaster work for one-offs.
  • Prepare the mould. Warm it until it is uncomfortably hot to hold (about 150 °C). Smoke the inside over a sooty flame of birch bark or pine resin; the soot stops the pewter sticking. Old pewterers brushed their metal moulds with a thin paste of fine pumice powder and egg white for the same purpose.
  • Pour steadily from a ladle, filling the mould in one go.
  • Finish. Pewter files, scrapes and burnishes easily. Turn plates and cups on a The Lathe with a sharp scraper, then polish with fine wood ash on a wet cloth. Pewter can also be hammered cold into shape over a wooden form, and it barely work-hardens, so it rarely needs annealing.

Method 4: Tinning iron and copper

Tinplate

Tinplate is thin iron sheet with a coat of tin on both sides. You need sheet iron about 0.3–0.5 mm thick (see Sheet Metal and Rolling), which is the hard part. The tinning itself is simple.

1 Grease pothot tallow dries the wet,clean sheet 2 Tin pottin at 300–330 °C under2–3 cm of tallow; 1–2 min 3 Finishing pottallow, about 240 °C;extra tin runs off evenly One long trench of embers under all three iron pots. Keep a lid and dry sand ready for grease fires.
Fig. 3 Making tinplate. Cleaned iron sheet passes through melted grease, then molten tin covered with grease, then grease again to smooth the coat.
  1. Clean the iron perfectly. Tin will only stick to bare, oxide-free iron. Scour the sheets with sand and water, then soak them in a sour liquid for several hours to a day to dissolve the last scale: historically, bran or rye meal fermented in water for a week (it turns sour), or vinegar. Later you can use dilute Sulfuric Acid — about 1 part acid to 20 parts water, always acid poured into water. Scrub again with sand, rinse, and keep the clean sheets under clean water until the moment you tin them, so they do not rust.
  2. Set up three iron pots in a row over a fire, or over one long trench of embers:
    • Grease pot: melted tallow (rendered beef or mutton fat), just hot enough to sizzle a drop of water.
    • Tin pot: molten tin at about 300–330 °C, with a layer of melted tallow 2–3 cm deep floating on top.
    • Finishing pot: melted tallow again, at about 240 °C.
  3. Dry and dip in grease. Take a sheet out of the water, dip it in the grease pot until it stops sizzling — this drives off the water and coats it in fat that keeps air away.
  4. Tin it. Lower the sheet edgewise slowly into the tin pot, through the grease layer, and hold it there for 1–2 minutes until it is as hot as the tin. Lift it out slowly and steadily.
  5. Smooth it. Dip it in the finishing pot for a few seconds. The excess tin melts and runs off evenly. Stand it on edge to drain.
  6. Clean off. When cool, rub the sheets with dry bran or sawdust to remove the grease.

Tinning a copper pot

Copper pots must be tinned inside before they are used for acid foods. Scour the inside bright with sand and vinegar. Heat the pot over a fire until a stick of tin rubbed on it just melts (about 240 °C — a drop of water dances and vanishes). Sprinkle in a little powdered pine resin (rosin) as a flux — a substance that cleans the surface and helps molten metal spread and stick. Rub the tin over the hot surface with a pad of cloth or tow until it melts and spreads in a bright, thin film over every part. Wipe off the excess while hot. Retin when copper shows through.

How to tell it worked

  • Tin cry. Bend a bar of pure tin near your ear: it makes a faint crackling sound. Pewter cries less.
  • Melting. Tin melts on the edge of a cooking fire; a drop on a cold stone sets with a bright, mirror-like surface. A dull, crinkled surface means impurities or overheating.
  • Bending. Refined tin bends easily without cracking. Raw tin that is hard and crumbly still contains iron: liquate it again.
  • Pewter. A pewter spoon should not bend in use, but should bend slowly, without breaking, under hard pressure.
  • Tinplate. The coat should be bright and smooth, with no bare grey spots. Wet a test piece with salt water and leave it overnight: well-tinned iron shows no rust, except at cut edges.

Note Troubleshooting. No tin from the furnace, just black glassy slag → ore too sandy, or fire not smothered enough. Clean the ore more, use more charcoal per charge, keep the furnace full. Tin freezes in the tap hole → keep the tap hole area hot by blowing occasionally across it, or put a few glowing coals in the basin. Tin hard and grey → iron in it. Liquate more slowly and gently. Pewter castings rough or incomplete → mould too cold, or metal too cool. Warm the mould more; check with the paper test. Tin will not stick to iron (bare spots) → the iron was not clean, or rusted after cleaning. Pickle longer; keep it under water; dip in grease before the tin. Grey powdery spots on tin left in hard frost → tin pest: below about 13 °C pure tin can very slowly change to a grey powder, fastest in long hard frosts. Pewter and tin with a trace of copper, antimony or bismuth resist it.

Dangers

Danger Hot grease fires. The tallow floating on the tin pot (300–330 °C) is hotter than tallow's flash point (about 265 °C): it smokes heavily, and its vapour catches fire from any flame or spark. Keep the tin no hotter than it needs to be, and keep open flame away from the surface. If it catches, never throw water on it — the water explodes into steam and sprays burning fat. Smother it with a close-fitting lid or a board, or with dry sand, and let it cool. Keep a lid and a bucket of dry sand beside the pots, and never leave them unattended.

Danger Molten metal and water. Sheets taken from water must be fully dried in the grease pot before they meet the tin. Water carried into molten tin explodes and throws metal. The same applies to furnace work: dry ground, dry moulds, no rain.

  • Arsenic and antimony fumes. Roast arsenic-bearing tin ore and smelt stibnite only in the open, upwind. White smoke is a warning: get out of it.
  • Lead. Keep lead out of pewter for food, and out of solder for drinking vessels and cans.
  • Acid. When pickling with sulfuric acid, always pour acid slowly into water, never water into acid, and protect your eyes. See Acids, Bases and Testing.
  • Burns. Molten tin does not glow, so it does not look dangerous. It is. Treat any pot of silvery liquid metal as if it were red-hot.

What this unlocks

Tin is half of Bronze and the main part of solder (see Soldering and Brazing). Tinplate gives you cans for Canning and Bottling (see Tins, Cans, Drums and Tanks), lanterns, funnels and pipes, and is the classic material for kitchenware (see Kitchen and Cooking). Tin with lead and antimony is type metal for Printing. Tin-lined copper pots make cooking safe. A thin tin foil backed with mercury was once used for Mirrors (see Mercury for why this is dangerous). Later, tin is needed for bearing metals (see Bearings and Lubrication) and is the usual coating for copper wire and electrical joints.

How it was first done

Tin was the rarest and most traded metal of the Bronze Age. Tin-bronze appears around 4,600 BC in the Balkans and became common across the Near East and Europe after about 3,000 BC; tin came from scattered sources in Anatolia, Central Asia, the Erzgebirge mountains of central Europe, Brittany and Cornwall. The Greek historian Diodorus, in the 1st century BC, described Cornish tinners smelting ore and carrying the metal to an island for trade. In medieval Cornwall and Devon, tin was smelted in small charcoal-fired shaft furnaces with water-powered bellows — the blowing houses — and tin was assayed and taxed in special "stannary" towns.

Pewter was made by the Romans, and in medieval Europe it became the common tableware of the middle classes; the Worshipful Company of Pewterers in London had its first rules by 1348, setting the allowed alloys. Tinplate was made in Bohemia and Saxony from the late Middle Ages, by dipping hammered iron sheet in tin. The Welsh works at Pontypool used rolled iron sheet from the 1720s, making tinplate cheaper. In 1810 Peter Durand patented the idea of preserving food in tin cans in England, and by 1813 Bryan Donkin and John Hall were supplying canned food to the Royal Navy.

Source: content/entries/metals/tin-and-pewter.md