◆ Rebuild

Part 6 · Building

Rot, Woodworm and Termites

Wood lasts for centuries if it is kept dry, and rots in a few years if it is not. How fungi and insects eat timber, how to tell dry rot from wet rot and old woodworm holes from live ones, how to design buildings that keep their timber dry and out of reach of termites, which preservatives to use (and which never to use), and how to cut out and repair damaged timber.

Difficulty
●●●●●
Time
An afternoon to inspect a building; a day to treat a roof with borax; days to weeks to cut out and splice decayed beams
Steps from zero
15 prerequisites →

You need first

Timber Framing and Log Building

This unlocks

—
The full path from nothing — 15 steps before this one
  1. Stone Tools
  2. Fire
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing
  13. Steel
  14. Axes, Chisels, Knives and Planes
  15. Timber Framing and Log Building
  16. Rot, Woodworm and Termites

Do them roughly in this order. See it on the tech tree →

Why it matters

Every timber house, barn, bridge, boat, fence and mine prop is food for something. A badly detailed sill beam can rot through in ten years; a well-detailed oak frame can stand for six hundred. Termites can hollow out the floor and roof of a house in the tropics in a few seasons without a single sign showing on the surface. A whole fleet of 18th-century warships rotted at their moorings before they ever sailed.

Most of this is preventable, cheaply, at the design stage. This chapter teaches how to:

  1. understand what wood-eaters need, so you can deny it to them;
  2. build so that timber stays dry and out of reach (Timber Framing and Log Building, Foundations and Floors, Roofs);
  3. recognise the damage, and tell whether it is still active;
  4. protect wood with preservatives you can make;
  5. repair what has been damaged.

Household pests that eat food and cloth — rats, moths, bed bugs — are in Household Pests. Creosote, the strongest preservative for posts in the ground, is in Coal Tar Chemicals.

How it works

Fungi: the real enemy

Rot is caused by fungi — the same family as mushrooms. Their spores are in every breath of air and land on every piece of wood. They only grow when four things are present together:

Need Detail What you do
Water Wood above about 20% moisture (by dry weight). Dry indoor wood is 8–15%; freshly felled wood is 40–200% Keep it below 20%. This is the whole game
Air Oxygen Wood that is always under water or deep in wet mud does not rot — Venice stands on wooden piles
Warmth About 5–40 °C, fastest at 20–30 °C (Little you can do)
Food Cellulose — the wood itself, especially sapwood Use naturally durable heartwood; poison the food with preservatives

Wood that is dry, or always wet, lasts. Wood that is sometimes wet — at ground level, at joints that trap rain, in a damp wall, under a leak — rots.

Three kinds of rot:

  • Brown rot eats the cellulose and leaves the brown lignin. The wood darkens, shrinks, and cracks across the grain into cubes; dry, it crumbles to brown powder between your fingers. Most rot in buildings is brown rot, including "dry rot" and the common cellar fungus.
  • White rot eats everything; the wood goes pale, soft, spongy and stringy. Mostly in hardwoods outdoors.
  • Soft rot softens the surface of very wet wood (posts in the ground, water tanks) to a soft grey skin that scrapes off.

Dry rot (the fungus Serpula lacrymans) is the most feared, because it does not stay where the water is. It grows from damp wood across brick, stone and plaster — sometimes metres — in grey strands as thick as a pencil, carrying water with it, to attack dry timber elsewhere. Its name is misleading: it needs damp to start, and it dies when the building is dried out. Wet rot (cellar fungus and others) needs wetter wood (40–50%) and stays close to the source of water.

Insects

Wood-boring beetles lay eggs in cracks in the wood. The larvae (grubs) tunnel inside for one to ten years, eating the wood and leaving powdery droppings (frass). Then they change into beetles and chew their way out, leaving the exit holes you see. By the time you see holes, the damage inside is years old — and the holes tell you only where adults left, not whether grubs remain.

Most beetles prefer sapwood (the pale outer wood of a tree, full of starch), and most prefer damp wood. Dry, heartwood timber in a dry building is rarely seriously attacked, except by the house longhorn and drywood termites in warm countries.

Termites ("white ants", though they are not ants) live in colonies of thousands to millions. Most kinds live in the soil and need moisture: they reach wood through the ground or through mud tubes they build up walls and foundations, and they eat the inside of timber while leaving a thin, unbroken outer skin. A few kinds (drywood termites, in warm coastal regions) live entirely inside dry wood.

What you need

Item Use
Knife or bradawl, light hammer Probing and sounding timber
Lamp or candle, mirror Looking into dark corners, under floors
Small scale or balance Moisture test (Measurement from Scratch)
Saws, chisels, augers, drawknife Cutting out and making repairs (Basic Woodworking, Axes, Chisels, Knives and Planes)
Props, jacks, wedges Supporting a frame during repair (Cranes and Lifting)
Borax (and boric acid if you can make it) Preservative for indoor and covered timber
Pine tar and linseed oil Surface protection outdoors (Tar, Pitch and Glue, Oils and Pressing)
Creosote Posts in the ground (Coal Tar Chemicals)
Lime Limewash and mortar (Lime)
Sheet metal (copper, zinc-coated iron) Termite shields, flashing (Sheet Metal and Rolling)
Coarse, hard crushed rock Termite particle barriers

Where to find it

Method 1: Build it dry

Good hatroof overhang 40–60 cm,gutter Downpipewater led well awayfrom the footings Good bootstimber 20–30 cm aboveground, clear of splash;bare masonry left visible Seasoned timberbelow 20% moisture Floor joistsover an airy crawl space Sill beamon a damp-proof course(slate, lead, tarred cloth) Termite shieldmetal, sticks out 4–5 cm,bent down at 45° Ventson opposite walls Particle barrier1.7–2.4 mm crushed rock
Fig. 1 Keeping timber dry and out of reach. A good hat (a wide overhang and gutter), good boots (a stone plinth with a damp-proof course), ventilation under the floor, drips and sloped tops on exposed wood, and in termite country a metal shield and a clear inspection gap.

The old rule is that a building needs good boots and a good hat.

  1. Season the timber before using it where it will be closed in. Air-dry it in stacks with spacer sticks, under a roof, open to the wind, for roughly a year for every 25 mm of thickness, until it is below 20% (Timber Framing and Log Building). Green oak frames are fine if open to the air so they dry in place; never box green timber into walls or floors.
  2. Lift it off the ground. Sill beams and posts stand on stone, brick or concrete footings at least 20–30 cm above the outside ground — high enough that rain splashing off the ground does not reach the wood (Foundations and Floors, Stone Masonry).
  3. Damp-proof course. Between masonry and timber, lay something water cannot climb through: a course of slate in mortar, a strip of sheet lead or copper, or a few layers of tarred cloth or birch bark. Masonry sucks water up from the ground like a wick; the damp-proof course stops it.
  4. Overhanging roof and gutters. Roofs should overhang walls by 40–60 cm, with gutters and downpipes that take water well away from the footings (Roofs).
  5. Ventilate under floors. A timber ground floor over a crawl space needs openings (air bricks, gratings) in the outer walls on opposite sides, every 1.5–2 m, kept clear, so air blows right through. Still, damp air under a floor is where dry rot begins.
  6. Shed water from every exposed piece. Cut the tops of posts and beam ends to a slope, or cap them with a board, slate or sheet metal. Undercut horizontal timbers with a drip groove so water falls clear. Never leave a hollow, upward-facing joint where rain can collect. Put the end grain — which drinks water like a bundle of straws — where it stays dry.
  7. Keep beam ends out of wet walls. Where a beam rests in a masonry wall, leave an air gap round its end, or sit it on slate, and make sure that part of the wall is not wet.
  8. Let it breathe. Use finishes that let moisture out: limewash, linseed oil, pine tar. Thick paint or tar on wood that gets wet from behind traps the water in and makes rot worse.
  9. Maintain. Clear gutters every autumn. Fix roof leaks at once. Most rot in old buildings starts at a blocked gutter or a slipped tile.

Method 2: Keep termites out

In termite country (most of the tropics and warm temperate lands), add these to Method 1:

  1. Clear the site of all stumps, roots, buried timber and scrap wood before building. Never bury wood offcuts or leave formwork in the ground.
  2. No wood touching soil. All timber at least 45 cm above ground in high-risk areas, on masonry or concrete.
  3. Leave an inspection gap. Keep at least 7–8 cm of bare foundation visible all round, free of soil, plants, steps and stacked firewood, so any mud tube crossing it can be seen.
  4. Termite shields (ant caps). On top of every pier and along the top of foundation walls, under the timber, set a continuous sheet of copper or galvanised iron that sticks out 4–5 cm and is bent down at 45°. Solder or fold every joint. Termites can build round a shield, but only in plain sight on its underside, where you will find and break the tube.
  5. Particle barrier. Termites cannot tunnel through a layer of hard, sharp grains too big for them to carry and packed too tight to squeeze between. Crushed granite or basalt sieved to between about 1.7 and 2.4 mm, laid 8–10 cm thick round foundations and under floors, works for decades. Sieve carefully: finer or coarser grains let them through.
  6. Resistant timbers where you can: heartwood of teak, cypress pine, some eucalypts, cedar.
  7. Inspect every few months: look for mud tubes on foundations, sound timbers by tapping, and look for discarded wings on windowsills after the first rains (a swarm).

Method 3: Preservatives

Preservatives poison the wood for fungi and insects. They work only as deep as they soak in, so put them on after all cutting and drilling, and on dry wood (except borax diffusion, below).

Preservative Best for How
Borax / boric acid Indoor and covered timber: roof timbers, floors, framing, furniture. Kills woodworm and fungi; very low danger to people Mix borax and boric acid 3 parts to 2 by weight and stir into hot water until no more will dissolve — roughly 100 g of the mixture per litre stays dissolved when warm, more when near boiling (borax alone dissolves far less). Brush or spray 2–3 coats on bare wood, applying it warm before crystals form. It washes out in rain: never use it in the ground or open weather
Borax diffusion Freshly sawn green timber Dip it in a hot, strong borax solution, then stack it tightly under a cover for 4–8 weeks: the borate soaks right through the wet wood
Creosote Posts and sleepers in the ground; bridges Hot-and-cold bath (Coal Tar Chemicals)
Pine tar with linseed oil Exposed outdoor wood above ground: cladding, shingles, boats, stave churches Thin hot pine tar with an equal part of linseed oil; brush on in warm, dry weather. Renew every 3–6 years (Tar, Pitch and Glue)
Copper sulfate (Boucherie method) Whole fresh-cut poles See below
Limewash Interior and exterior walls and timbers Mildly antiseptic and insect-deterring, and bright; mainly hygiene (Lime)
Charring Post ends, cladding Burning the surface to a black crust protects against weather and some insects; it does not stop rot in the ground on its own

The Boucherie method (for poles). Within a day or two of felling, while the sap still runs, stand the pole butt-up, or lay it sloping. Tie a tight leather or rubber cap over the butt end, and feed it from a tank set 5–10 m above with a 1–2% solution of copper sulfate (10–20 g per litre). Over several days the solution pushes the sap out of the far end; stop when the liquid dripping out is as blue as the feed (a clean iron nail dipped in it comes out copper-coated). Never taste it: copper sulfate is poisonous. Copper-treated poles last two to four times longer in the ground.

Making boric acid. Dissolve borax in the least possible boiling water, add Hydrochloric Acid or Sulfuric Acid slowly until a drop turns blue litmus red, and let it cool: shiny white flakes of boric acid crystallise out. Rinse them with a little cold water.

Warning Preservatives never to use. Arsenic (as in the old "CCA" green-treated timber, see Arsenic), mercury chloride ("kyanising"), pentachlorophenol and the old organochlorine insecticides all work, and all poison people, animals, soil and water for generations. Do not make them, and never burn or reuse wood treated with them.

Recognising the damage

Beetle exit holesdrawn about 3 times actual size Furniture beetleround 1.5–2 mmgritty pellets Powderpostround 1–1.5 mmflour-fine dust Death-watchround about 3 mmbun-shaped pellets House longhornoval 6–10 mmpacked in tunnels Rot and termites Brown rotdark, shrunk, cracked into cubes;crumbles to powder when dry Dry rotwhite cottony sheets, grey strandsacross brick, rust-red fruiting bodyand red-brown dust; mushroom smell Mud tubepencil-wide, upthe foundationthin skin, hollow insideTermitestimber sounds hollow; layeredgalleries packed with soil;shed wings on sills after rain Fresh beetle holes have clean, pale edges and fresh frass below them; old holes are dark and dusty.
Fig. 2 What the damage looks like. Exit holes and frass identify the beetle; brown cubes, white sheets and grey strands identify rot; mud tubes and thin-skinned hollow timber mean termites.

Rot.

  • Probe: push a knife point into the wood across the grain and lever up a splinter. Sound wood lifts a long, fibrous splinter that breaks with a crack. Rotten wood lets the knife sink in easily and breaks off short and brittle ("brash"), or is soft and spongy.
  • Sound: tap with a hammer. Sound timber rings; decayed timber sounds dull or hollow.
  • Look and smell: brown cubes and cracks across the grain (brown rot); pale, stringy, soft wood (white rot); white cotton-wool growth, grey strands over brick, a flat rust-red fruiting body like a pancake with a white edge, and fine red-brown dust (dry rot); a damp, mushroomy smell.
  • Moisture: cut a sliver from the suspect wood, weigh it at once, dry it on a warm stove or in an oven at about 100 °C until it stops losing weight, and weigh again. Moisture % = (wet weight − dry weight) ÷ dry weight × 100. Over 20%: rot can grow. Over 30%: it is growing.

Beetles.

Beetle Exit hole Frass (droppings) Where
Common furniture beetle (woodworm) Round, 1.5–2 mm Gritty, cream; tiny lemon-shaped pellets Sapwood of any wood; damp floors, furniture, roofs
Powderpost beetle Round, 1–1.5 mm Fine as flour Sapwood of new oak, ash, elm and other starchy hardwoods, in the first years after sawing
Death-watch beetle Round, about 3 mm Bun-shaped pellets visible to the eye Old oak and elm, always with damp and fungal decay; adults tap loudly in spring
House longhorn Oval, 6–10 mm, ragged Sausage-shaped pellets packed in tunnels Softwood sapwood in roofs, in warm regions; grubs can be heard scraping. Serious
Wood-boring weevil Small, ragged Fine Only in wet, already rotten wood — treat the rot

Is it still alive? Fresh exit holes have clean, pale edges; old ones are dark and dusty inside. Small heaps of fresh frass under holes mean activity. In spring, paste thin paper over a patch of holes, or rub the patch with wax or paint: new holes punched through it by summer prove a live infestation.

Termites. Earthen mud tubes, about a pencil wide, running up foundations, piers or walls; timber that sounds hollow and crushes under a thumb, with layered galleries packed with soil inside; swarms of winged insects after rain and their shed wings on sills. Drywood termites push out tiny, hard, six-sided pellets like coarse sand or poppy seed that pile up below a kick-out hole.

Method 4: Treatment and repair

  1. Find and stop the water. Nothing else works without this. Fix the gutter, the leak, the blocked vent, the soil heaped against the wall. Let the building dry out; open it up and air it.
  2. Find the extent. Probe and sound every timber near the trouble. For dry rot, follow the strands through walls and under floors to their end.
  3. Prop first. Before cutting out any structural timber, support the load above it with props and wedges or jacks (Cranes and Lifting, Scaffolding and Ladders).
  4. Cut out the decay. Cut back to sound wood. For dry rot, cut 30–60 cm beyond the last visible sign, take down affected plaster, strip strands off masonry, and treat the masonry with hot borax solution or heat it with a brazier where safe. Burn the removed wood.
  5. Treat sound timber nearby with borax, two to three coats.
  6. Splice in new timber. Use well-seasoned, durable heartwood. Join it to the old with a scarf joint — a long, sloping lap at least 3–4 times the beam's depth long — pegged with oak pegs or through-bolted (Doors, Windows and Joinery, Screws, Nuts and Bolts). Where you cannot cut out, sister the beam: bolt a new beam, or a pair of planks, alongside the weak one.
  7. Insects. Dry the timber, then brush borax on all bare surfaces. Heat kills every insect stage: wood held at 56 °C right to its core for 30 minutes is clean; small pieces and furniture can be heated in a sealed hot room, a bread oven cooling down, or a black-painted box in strong sun. Freezing small items at −20 °C for one to two weeks (in a hard winter, outdoors in a closed box) works too. Cut out and replace timbers that are badly weakened; leave the old holes otherwise — most are history.
  8. Termites. Break all mud tubes and check daily for rebuilding to find the route. Replace damaged timber with resistant wood on proper shields. For mound-building species, dig out the mound down to the royal chamber and destroy the queen; the colony then dies.
  9. Watch. Mark any crack with a dated pencil line, look again each season, and keep a record.

How to tell it worked

  • Moisture of the repaired timber falls below 20% and stays there through a wet season (weigh-and-dry test).
  • No fresh frass, no new holes through papered patches the following summer.
  • No rebuilt mud tubes across the inspection gap or on the shields for a year.
  • No new white growth, strands or mushroom smell where dry rot was cut out.
  • Probed timbers give long splinters, and tapped beams ring.

Note Troubleshooting. Rot keeps returning after repair → the water source was not found or fixed. Look higher: rot is often fed by a leak far above it. Borax-treated timber rotted outdoors → borax washes out in rain. Use creosote or tar outdoors, and keep borax for covered timber. Creosoted post rotted at ground level → it was cut or notched after treatment, or the wood was wet when treated and took up little oil. Mud tubes appear above the shield → a joint in the shield is open, or something (a step, a plant, a pipe) bridges it. Seal joints and clear the gap. New wood in an old frame shrank and the joint opened → the new timber was not seasoned. Use dry wood for repairs, or tighten the joint after a year. Damp still rising in a wall → no damp-proof course, or soil piled above it. Lower the soil outside, add a drain trench filled with gravel along the wall.

Dangers

Danger Collapse during repair. A rotten beam may be carrying a floor, a roof or a wall. Prop everything above it before cutting, keep people out from under it, and never stand on a floor or roof you have not tested. Many rotten floors look sound until a foot goes through.

  • Hidden rot overhead. Rotten roof timbers can drop slates, tiles or a whole section of roof. Check ceilings for sagging and stains before working under them.
  • Mould and spores. Clearing heavy rot and mould raises clouds of spores. Wet the material first, cover mouth and nose, and work with windows open.
  • Preservatives. Creosote burns the skin and causes cancer (Coal Tar Chemicals); copper sulfate and boric acid are poisonous if swallowed — keep them away from children, animals and food. Never burn treated timber on a cooking or house fire.
  • Termite mounds can hide snakes. Approach with a stick and boots.

What this unlocks

Timber buildings, bridges and boats that last generations instead of decades (Timber Framing and Log Building, Roads and Bridges, Boats and Sails); durable fence posts (Fences and Hedges), poles for the The Telegraph and Power Lines and Distribution, railway sleepers (Railways) and mine props (Mining and Tunnelling); safe storage of grain and goods (Granaries and Food Storage).

How it was first done

People have known for thousands of years which woods last: the Roman engineer Vitruvius praised larch and oak and advised felling timber in autumn and seasoning it before use. Norwegian stave churches, coated with pine tar renewed for centuries, still stand from the 1100s and 1200s, and Venice has stood since the Middle Ages on wooden piles driven into waterlogged mud. In the 1700s and early 1800s dry rot was a crisis for the British navy: ships built of unseasoned timber rotted in harbour, and some needed rebuilding before they ever went to sea. The search for cures produced the first industrial wood preservatives: John Kyan's mercury chloride (1832), and in 1838 William Burnett's zinc chloride, John Bethell's pressure creosoting and Auguste Boucherie's copper sulfate sap-displacement. Henry Smeathman described the termites of West Africa to the Royal Society in 1781. Between 1914 and 1923 the 14th-century oak hammerbeam roof of Westminster Hall in London, riddled by death-watch beetle, was saved by hidden steel reinforcement.

Source: content/entries/building/wood-decay-and-pests.md