◆ Rebuild

Part 2 · Earth and Fire

Ore Dressing: Jigs, Tables and Flotation

Most ore as it comes out of the ground is mostly worthless rock. Ore dressing turns it into a rich concentrate before smelting, by hand picking, by washing in jigs and on shaking tables that let heavy grains sink, by magnets, and by froth flotation, where oiled metal minerals ride air bubbles to the top. Then the water is recovered in thickeners and the waste stored safely behind a tailings dam.

Difficulty
●●●●●
Time
A day to build a hand jig and test an ore; weeks to build and tune a shaking table and a bank of flotation cells; a tailings dam is built over the whole life of the mine
Steps from zero
23 prerequisites →

You need first

Ball Mills, Crushers and GrindersMining and Tunnelling

This unlocks

—
The full path from nothing — 23 steps before this one
  1. Fire
  2. Stone Tools
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Simple Machines
  7. Basic Woodworking
  8. Hunting and Trapping
  9. The Kiln
  10. Charcoal
  11. Pottery
  12. Quarrying and Cutting Stone
  13. Hides and Leather
  14. Lime
  15. Mining and Tunnelling
  16. The Wheel and Axle
  17. Portland Cement
  18. Bellows
  19. The Lathe
  20. Copper Smelting
  21. Bronze
  22. Bearings and Lubrication
  23. Ball Mills, Crushers and Grinders
  24. Ore Dressing: Jigs, Tables and Flotation

Do them roughly in this order. See it on the tech tree →

Why it matters

A smelter wants rich ore: the bloomery turns poor ore entirely into slag. But rich ore runs out first, and every later mine faces rock with a few percent of metal or less, its grains scattered like raisins in bread.

Ore dressing (also called mineral processing) separates the valuable mineral from the waste rock before any fuel is burned. It makes lead, zinc, copper, tin, tungsten and Molybdenum possible on any scale, and the same skills clean coal, purify sand for Glass and recover diamonds and zircon.

How it works

First free the grains (liberation). Crushing and grinding (Ball Mills, Crushers and Grinders) must break the rock small enough that most grains are either mineral or waste, not both stuck together. Look at crushed ore under a lens: when most metal grains are loose and clean, you have ground enough. Coarse tin and galena ore frees at 1–3 mm; most copper and zinc sulfide ores only as flour, most of it through a 200-mesh sieve (0.075 mm). Never grind finer than needed: it costs power and makes slime that is hard to recover.

Then sort by a property that differs.

Property Method Works for
Colour and shine Hand picking Coarse, rich ore
Weight for size (density) Panning, sluices, jigs, tables, buddles Tin, tungsten, lead, gold, iron sands, coal
Magnetism Magnets and separators Magnetite, wolframite, ilmenite, garnet
Whether water wets the surface Froth flotation Copper, lead and zinc sulfides, molybdenite, graphite, coal
Electric conductivity Electrostatic separator (Zircon and Zirconium) Mineral sands

Words you need. The feed goes in; the concentrate is the rich product; the tailings are the waste; middlings are in-between grains, reground and fed again. Grade is the percentage of metal in a product; recovery is the share of all the metal in the feed that ends up in the concentrate. The two fight: a richer concentrate means more metal thrown away.

A worked example. 100 t of ore at 2% copper holds 2 t of copper. Recover 90% of it into a concentrate of 25% copper, and the concentrate weighs 2 × 0.9 ÷ 0.25 = 7.2 t; the 92.8 t of tailings still hold 0.2 t (about 0.2%). Assay all three to check yourself (Gold and Silver, Identifying Substances).

Gravity separation needs contrast. In water each grain is buoyed up, so what counts is its density minus one. Densities (times water): quartz and calcite 2.65; sphalerite and chalcopyrite 4.0–4.2; molybdenite 4.7; pyrite, magnetite and hematite 5.0–5.3; scheelite 6.0; cassiterite, wolframite and galena 7.0–7.5; gold and platinum 15–19. Divide the heavy mineral's figure by the light one's. Galena in quartz: (7.5 − 1) ÷ (2.65 − 1) = 3.9, easy at almost any size. Chalcopyrite in quartz: 3.2 ÷ 1.65 = 1.9, possible only on coarse, evenly sized grains. Below about 1.25, gravity will not work at all. That is why copper and zinc sulfides need flotation.

Mine Hand picking Crush and grind Screen and classify waste rock to the heap coarse, 1–12 mm sand, 0.05–2 mm flour, under 0.1 mm Jigs Shaking tables Flotation cells Thickener Filter, then to the smelter Tailings dam concentrates tailings (waste sand and slime) clear water from the dam and thickener goes back to the mill
Fig. 1 A dressing plant. Ore is hand-picked, crushed and ground, then sized. Coarse heavy minerals go to jigs, fine sand to shaking tables, the finest flour to flotation cells. Concentrates are dewatered in a thickener; tailings go behind a dam, and clear water returns to the mill.

What you need

Item Notes See
Crushers, mills, sieves To free the grains and size the feed Ball Mills, Crushers and Grinders
Water, 5–20 tonnes per tonne of ore Recycle it Dams and Reservoirs
Timber, planks, pitch, wire cloth Jig boxes, tables, launders (open wooden channels for slurry) Basic Woodworking, Iron and Brass Wire
Cams, cranks, belts and a water wheel or engine Driving jigs and tables Cranks, Cams and Linkages, The Waterwheel
Electromagnets Magnetic separation The Electromagnet
Pine oil, paraffin or creosote oil, lime Flotation Below
A gold pan and a balance Testing every product Finding and Identifying Ores, Balances, Steelyards and Weighing Machines

Hand picking

The oldest step and still the first. Wash the broken ore so colours show — under a spray, or in a turning drum of screen (a trommel) — and sort it by eye.

  1. Cobbing. On a hard spalling floor of stone or iron plate, break fist-sized lumps with a 1–2 kg hammer and knock the waste off the ore. Throw clean ore, mixed pieces and waste into separate heaps.
  2. The picking table. For a larger mine, a slow belt 60–90 cm wide, moving at a slow walking pace (0.15–0.3 m a second), or a round, slowly turning iron table 2–4 m across, with pickers standing alongside. Feed only lumps of 2–10 cm; smaller pieces go straight to the mill. Light it well from above. A picker removes 1–2 tonnes of waste an hour. Scheelite is picked in the dark under ultraviolet lamps (Tungsten and Filament Wire).

The ore jig

A jig lets heavy grains sink through a bed of sand that is lifted and dropped by pulses of water. On each upward pulse the bed loosens; as it settles, heavy grains drop faster and work their way down while light ones stay on top.

The hand jig

  1. The tub: a barrel or water-tight tub about 1 m across and 80 cm deep, full of water.
  2. The sieve: a wooden hoop 50–60 cm across and 15–20 cm deep with a bottom of wire cloth or punched iron, holes 2–3 mm, hung from one end of a lever pole pivoted on a post.
  3. Size the feed first: jig only a narrow range, such as 3–6 mm or 6–12 mm. Mixed sizes do not separate.
  4. Jig. Fill the sieve two-thirds full. Plunge it sharply down and lift it gently, 60–100 strokes a minute, each 3–6 cm, keeping it level.
  5. Skim. After 1–3 minutes the sieve holds layers: waste on top, middlings, heavy ore at the bottom; the finest heavy grains have fallen into the tub. Scrape the layers off in turn with a flat wooden blade.

The plunger jig

Plunger jig (section) Shaking table (from above) sized ore and water light waste over tailboard Plunger 1–4 cm stroke, 120–300 a minute Partition Screen with heavy ragging Hutch heavy product out at the spigot feed wash water slow forward, snap back: 250–300 a minute tilt down Concentrate dark streak, far end Middlings Tailings wash off the low side Head riffles taper to nothing along the dashed line
Fig. 2 Left, a plunger jig in section. A plunger pumps water up and down through a screen holding the ore bed; heavy grains sink through the ragging into the hutch, light grains wash over the far end. Right, a shaking table from above: the deck jerks along its length while water flows across it, and grains fan out into concentrate, middlings and tailings.
  1. The box: a water-tight wooden or steel tank divided lengthways by a partition that stops 15–20 cm short of the bottom. One side holds a flat wooden plunger that nearly fills it; the other a horizontal screen, 40 × 80 cm to 60 × 100 cm. Below the screen the box narrows to a pointed hutch with a plugged outlet (spigot).
  2. The drive: an eccentric gives the plunger a stroke of 1–4 cm at 120–300 strokes a minute — short and fast for fine feed, long and slow for coarse.
  3. Feed sized ore and water at one end. Light waste washes over a low tailboard at the far end.
  4. Heavy product. For coarse feed, let it out through a side gate just above the screen. For feed under 2–3 mm, cover the screen with ragging — heavy pieces bigger than the screen holes, such as galena lumps or iron shot — through which fine heavy grains work down into the hutch and out at the spigot.
  5. Hutch water: a little clean water fed into the hutch softens the suction on the down-stroke.

A two- or three-compartment jig treats 1–5 tonnes an hour.

Good versus bad. The bed should breathe, rising and falling evenly over the whole screen. A bed that never loosens is too tight (more water, longer stroke); one that boils and throws grains about is too loose. Pan a handful of tails every hour.

The shaking table

A table separates fine sand, 0.05–2 mm, too fine to jig. It is the most precise gravity machine there is.

  • The deck: a flat rectangular board, full size about 4.5 × 1.8 m; a small one 2 × 0.8 m treats a few hundred kilograms an hour. Cover it with linoleum or rubber (Linoleum, Oilcloth and Floorcloths, Rubber).
  • Riffles: thin wooden strips along the length, 3–4 cm apart, 1–1.5 cm high at the feed end, tapering to nothing along a diagonal line across the deck.
  • Tilt: 2–6° sideways, down from the feed side to the tailings side, set with wedges. Lengthways, level or rising very slightly toward the concentrate end.
  • The head motion is the secret: the deck moves slowly forward and snaps back, 250–300 times a minute, stroke 10–25 mm. Grains in the riffles ride the slow push and slide on when the deck stops. The simplest drive: a cam draws the deck back against a strong spring and releases it; the spring throws it forward against a padded bumping post. Mount the deck on short rockers or greased slides.

Running it.

  1. Feed slurry of 20–25% solids by weight (one bucket of sand to three of water) at the upper corner.
  2. Run wash water from a perforated pipe along the upper side so a thin film crosses the deck.
  3. Watch the fan. A dark streak of heavy mineral travels along the riffles to the far end (concentrate); light quartz washes over the low side (tailings); middlings come between. Movable splitters in the launder under the edges divide them.
  4. Adjust one thing at a time: more tilt or water gives a cleaner concentrate and more loss; less gives more recovery and a dirtier concentrate.

A well-tuned table shows a knife-sharp line between the dark streak and the pale sand.

The buddle

For slime too fine for tables, the Cornish round buddle is cheap: a shallow circular pit 5–7 m across, lined with planks or smooth clay, sloping outward from a central cone 1 m across. Slurry fed on the cone spreads out in a thin sheet; the heaviest grains settle nearest the centre, the lightest at the rim, while slowly turning brushes smooth the surface. When the deposit is 20–30 cm deep, dig it out in rings: inner ring concentrate, middle ring re-buddled, outer ring waste.

Magnetic separation

  • The hand magnet. A lodestone or steel magnet wrapped in paper, drawn over dry sand, lifts magnetite. Pull the paper off over a dish and the grains fall.
  • The wet drum separator for magnetite: a drum of wood or brass sheet, 40–90 cm across, turning at about 1 metre a second at its surface, with fixed magnets inside covering a third of its circle on the side that dips into the slurry. Magnetite clings, is carried over the top, and drops off where the magnets end.
  • The cross-belt separator for weakly magnetic minerals (wolframite, ilmenite, garnet): dry, sized grains ride a belt under strong electromagnets with sharp, wedge-shaped poles 3–10 mm above it (The Electromagnet). A second belt runs crosswise just under each pole and carries off the grains that jump up. Weak poles first, then stronger.
  • Magnetising roast. Roast hematite or siderite at 500–700 °C with 3–5% charcoal and little air: it becomes magnetite, which a drum can pick up.

Froth flotation

Close up: oiled grains cling to the bubble; wet quartz does not Conditioned pulp ore, water, reagents Motor 400–700 turns a minute Air drawn down the standpipe Paddles Froth over the lip into the launder: concentrate Tail gate sets the pulp level; tailings to next cell Impeller 15–25 cm across Stator calms the swirl Quartz sinks stays in the pulp
Fig. 3 A flotation cell. A spinning impeller near the bottom sucks air down the standpipe and breaks it into fine bubbles. Oiled mineral grains stick to the bubbles and rise into a froth, which overflows the lip into a launder. Wetted quartz stays in the pulp and leaves through the tail gate.

This one process recovers most of the world's copper, lead, zinc and molybdenum, from grains too fine and too light for any table.

How it works. Water wets quartz and most rock. It does not wet a sulfide grain given a thin coat of an oily chemical: water pulls back from it as from a greased pan. Blow fine air bubbles through the slurry and the water-repelling grains stick to them and rise. A frother keeps the bubbles small and makes them build a froth that holds its load at the surface. Skim the froth: that is the concentrate.

Reagent What it does What to use Amount per tonne of ore
Frother Small, stable bubbles Pine oil (steam-distilled from pine stumps or [[pine resin resin]], Distillation); cresylic acid from coal tar (Coal Tar Chemicals)
Collector Makes the wanted mineral repel water Paraffin or fuel oil (Petroleum and Refining), creosote oil; better, xanthate Oil 0.2–2 kg; xanthate 20–150 g
Lime Raises pH to 9–11, stops pyrite floating Slaked Lime 0.5–3 kg
Activator Lets sphalerite float after the lead is out Copper sulfate (Copper Smelting) 100–500 g
Depressant Holds one mineral down Zinc sulfate holds back sphalerite while galena floats; starch holds back graphite and talc; Water Glass (Sodium Silicate) keeps clay slime dispersed 100–1,000 g

Molybdenite, graphite, sulfur and coal float with oil and frother alone, being naturally water-repelling; galena floats readily with a little oil. Start with these. Xanthate, the best sulfide collector, is made from alcohol, caustic potash and carbon disulfide (sulfur vapour passed over red-hot charcoal, as for viscose in Rayon and Nylon); leave it to a works with chemical training. Oil flotation works without it, at lower recovery.

The flotation cell

  1. The tank: a wooden or steel box 40–60 cm square and 50–70 cm deep, with a front lip and a launder below it.
  2. The impeller: a disc 15–25 cm across with short vanes underneath, 3–5 cm above the floor, turning at 400–700 revolutions a minute. Around its shaft a standpipe open to the air: the spinning impeller sucks air down it and tears it into fine bubbles. A ring of fixed vanes round the impeller (the stator) calms the swirl so the surface stays quiet.
  3. Paddles turning slowly along the lip scrape froth into the launder; an adjustable tail gate on the far side sets the pulp level.

The simplest cell is a barrel with a canvas bottom and air blown up through it by a fan (Centrifugal Pumps and Fans); the canvas clogs, but it works. Cells are set in a row, the tailings of each flowing to the next: roughers first, scavengers last to catch what was missed, and cleaners to float the rough concentrate again for a higher grade.

The bucket test

  1. Grind 1 kg of ore wet with 1 litre of water until most passes 200 mesh. Pour it into a bucket and add water to about 3 litres.
  2. If pyrite is present, add lime to pH 9–10 (red cabbage paper, pH, Indicators and Buffers).
  3. Add 2–3 drops of paraffin oil or creosote and stir 5 minutes. Add 1–2 drops of pine oil and beat hard with a whisk so air is drawn in.
  4. Skim the froth into a pan for 5–10 minutes, until it turns white and empty. A good froth is grey to black and metallic, thick with grains.
  5. Dry, weigh and pan both products. The tailings should pan almost clean.

Tip A froth that is white and empty wants more collector. One that is stiff and won't break has too much frother. Big, bursting bubbles need more frother or a faster impeller.

Thickeners and water

Concentrate and tailings leave as slurries that are mostly water, which you want back.

The thickener is a round tank 3–30 m across and 2–4 m deep, its floor sloping gently to a central cone. Slurry enters a feed well in the middle; solids settle; clear water flows over a weir all round the rim and back to the mill. Rake arms on a central shaft turn once every 5–30 minutes, their tips moving only 3–8 m a minute, pushing settled mud to the cone, where a pump draws it off at 50–65% solids. Too fast a rake stirs the mud back up.

Size it by test: time how fast the line between clear water and mud falls in a tall jar of slurry; the slower, the more floor you need. A little lime, starch or glue makes fine mud settle many times faster. As a rough start, a concentrate needs 0.2–0.5 m² of floor for each tonne of solids a day; slimy tailings several times more. A filter press or vacuum drum filter then takes concentrate down to 8–12% moisture.

The tailings dam

Almost all the ore you mine ends as tailings — fine, wet sand and slime with traces of poisonous metals — and it must be stored safely forever.

Dry beach, 50–100 m keeps the pond away from the wall Spigots on the crest Pond Decant tower water back to the mill Tailings fine sand and slime seepage out Starter dam compacted earth, clay core Raises built downstream outer side, never on tailings Toe drain gravel height exaggerated for clarity
Fig. 4 A tailings dam in section. A compacted earth starter dam with a clay core and a gravel toe drain holds the tailings. Each raise is built downstream, on the outer side. Tailings are spread from the crest so a wide beach keeps the pond far from the wall; clear water is drawn off by a decant tower and returned to the mill.
  1. Site it in a valley or basin not above any village, road or water supply, never across a stream. Dig ditches to lead rain and stream water around it.
  2. Build a starter dam of compacted earth 3–5 m high, with a puddled clay core and a gravel toe drain at its outer foot to let seepage out without washing the dam away (Dams and Reservoirs). Outer slope no steeper than 1 in 3.
  3. Spread tailings from the crest, so coarse sand settles near the wall as a beach and slime and water collect far off in a pond. Keep 50–100 m of dry beach between pond and wall.
  4. Draw off water through a decant tower of stacked boards or concrete rings with a pipe under the dam, and pump it back to the mill. Keep 1–2 m of freeboard and a spillway for floods.
  5. Raise it downstream: build each new layer on the outer side, on the old dam and solid ground. Never build raises inward on top of the soft tailings (the cheap upstream method): shaken or soaked, those tailings can turn liquid and the whole wall fails at once.
  6. Close it with clay, soil and grass. Keep pyrite-rich tailings wet or sealed: dry pyrite makes acid that leaches metals into streams for centuries. Crushed limestone in the drains neutralises it.

Warning signs: seepage or muddy water from the outer face or toe, cracks along the crest, the pond creeping toward the wall. Stop feeding, lower the pond and repair at once.

How to tell it worked

  • Pan every product every shift. Concentrate is mostly heavy mineral; tailings show only a speck.
  • Weigh and assay feed, concentrate and tails daily. Metal in the feed should equal metal in concentrate plus tails.
  • Recovery to aim for: tin and tungsten by gravity 60–80%; galena by jigging 85–95%; copper sulfide by flotation 85–95%.

Note Troubleshooting. Heavy mineral in jig tails → feed too fast or badly sized, stroke too long. Table concentrate dirty → too little tilt or water, feed too thick. Mineral lost as slime → overground; grind coarser and classify out fines before regrinding. Froth full of pyrite → raise the pH with lime. Poor flotation recovery → grains not freed (grind finer), tarnished oxidised ore (use fresh ore), or too little collector. Thickener overflow cloudy → feeding too fast; add lime or starch.

Dangers

Danger Tailings dam failure is one of the deadliest industrial disasters. A burst dam releases liquid mud that moves faster than people can run and buries everything below. Never build upstream raises, never let the pond reach the wall, never site a dam above homes, and inspect it after every heavy rain and earthquake.

Danger Carbon disulfide (for xanthate) catches fire from a hot steam pipe without any flame, and its vapour poisons the nerves and brain. Do not make it without training and closed apparatus.

  • Machinery: jig cranks, table heads, belts and impellers catch clothing and limbs. Guard them; stop the drive before reaching in.
  • Dust from dry crushing and dry magnetic work: silica and lead (Ball Mills, Crushers and Grinders). Keep everything wet that can be.
  • Reagents burn skin and eyes (pine oil, cresylic acid, lime) or poison (copper sulfate, lead minerals).
  • Drowning and poisoned water: fence thickeners and ponds, whose soft bottoms trap a person, and never let people or livestock drink tailings water.

What this unlocks

Rich concentrates for every base-metal smelter: Copper Smelting, Lead, zinc, tin, Nickel and Cobalt, Tungsten and Filament Wire and Molybdenum. Clean coal (Coal and Coke), pure sand for Glass and Optical Glass and Achromatic Lenses, mineral sands for Titanium and Zircon and Zirconium, graphite for crucibles and pencils, and platinum grains from the gold pan (Platinum and the Platinum Metals). Copper ore too poor or too oxidised to float can instead be leached with dilute acid, with no furnace at all (Leaching, Solvent Extraction and Electrowinning).

How it was first done

Hand picking and washing are as old as mining. Georgius Agricola's De re metallica (1556) shows jigging sieves, washing tables and buddles worked by water power in central Europe. Cornish and German mines of the 19th century refined the round buddle and the Harz plunger jig; Peter von Rittinger in Austria built a bumping table in the 1850s, and Arthur Wilfley of Colorado patented the riffled shaking table in 1896. John Price Wetherill's strong magnetic separator of 1896 handled weakly magnetic minerals.

Francis and Stanley Elmore in England patented oil flotation in 1898. At Broken Hill, Australia, around 1903–1905, Charles Potter, Guillaume Delprat and the company Minerals Separation developed froth flotation to recover zinc from millions of tonnes of old tailings, and Cornelius Keller introduced xanthate in 1923. John Van Nostrand Dorr invented the raked thickener in 1906. Tailings-dam failures — Stava in Italy (1985) and Brumadinho in Brazil (2019), each killing about 270 people — are why the rules above are strict.

Source: content/entries/earth/ore-dressing.md