Magnesium

The lightest metal you can build with, a third lighter than aluminium. It lies dissolved in every bucket of seawater and locked in dolomite rock, but only electricity can free it. This chapter covers the easy magnesium compounds first — Epsom salt, magnesia, magnesia cement — then making the metal by electrolysis of molten magnesium chloride, its uses, and its fierce fires.

Difficulty
●●●●●
Time
A week to make Epsom salt and magnesia from bittern; months to build and run a molten-salt cell
Steps from zero
16 prerequisites →

You need first

ElectrolysisSalt

This unlocks

Titanium
The full path from nothing — 16 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Pottery
  10. Hides and Leather
  11. Salt
  12. Fermentation
  13. Bellows
  14. Copper Smelting
  15. The Battery
  16. Electrolysis
  17. Magnesium

Do them roughly in this order. See it on the tech tree →

Why it matters

Magnesium metal weighs 1.74 g per cubic centimetre — two-thirds of aluminium, less than a quarter of steel. Alloyed with a little aluminium and zinc it is strong enough for wheels, engine cases, tool bodies and aircraft parts. But its most important jobs are quieter:

  • Fixing other metals. A few hundredths of a percent of magnesium stirred into molten The Blast Furnace and Cast Iron turns the graphite inside it from sharp flakes into round balls. Brittle cast iron becomes ductile iron, which bends instead of snapping — good enough for crankshafts, pipes and gears. Magnesium also hardens aluminium alloys (Aluminium).
  • Pulling oxygen out of things. Magnesium grabs oxygen and chlorine more strongly than almost any other metal. Heated with the chlorides of titanium, zirconium or uranium, it strips them out as metal. It removes sulfur from steel. In a The Vacuum Tube, a speck of it flashed onto the glass soaks up the last traces of gas (a getter).
  • Protecting iron. A block of magnesium bolted to a steel hull, a buried pipe or the inside of a water heater corrodes away instead of the steel — a sacrificial anode (Corrosion and Its Prevention).

Its compounds are easier and just as useful. Magnesia (magnesium oxide) is a refractory that stands 2,000 °C and more (Firebrick and Refractories). Epsom salt is a laxative, a soak for sprains, and a fertiliser for magnesium-starved crops (Chemical Fertilisers). Magnesia mixed with magnesium chloride sets to a hard, smooth stone (Sorel cement) for floors and grindstones.

Be honest about the metal: it needs a molten-salt electrolytic cell running at about 700 °C, thousands of ampere-hours per kilogram, and dry chlorine handling. Do the compounds first. Make the metal when you already make Aluminium or run a chlor-alkali works (Electrolysis).

How it works

Magnesium is everywhere but never alone. Seawater holds about 1.3 g of magnesium per litre — after sodium, the most plentiful metal in the sea. Dolomite rock is half magnesium carbonate; magnesite is nearly all magnesium carbonate.

Three chemical facts drive everything:

  1. Lime throws magnesium out of seawater. Magnesium hydroxide hardly dissolves at all. Stir slaked Lime (calcium hydroxide) into seawater and the magnesium comes down as a fluffy white sludge, while the calcium takes its place in the water.
  2. Water cannot be used to free the metal. Magnesium is so eager to combine that in a water solution the current makes hydrogen, not metal. So you must melt a dry magnesium salt and electrolyse the melt, as for aluminium. The cell runs at 700–750 °C, just above magnesium's melting point of 650 °C. Molten magnesium is lighter than the molten salt and floats to the top at the cathode, while chlorine gas bubbles off the carbon anode.
  3. Drying the chloride is the hard part. Magnesium chloride crystallises with six molecules of water. Heat it in air to drive the water off, and it reacts with its own water instead, giving off hydrogen chloride fumes and leaving useless magnesium oxide. It must be dried slowly in a stream of dry hydrogen chloride gas, or only partly dried and fed hot into the cell.

Faraday's law (Electrolysis): each magnesium atom needs two electrons, so 1 kg of magnesium needs about 2,200 ampere-hours. At 6–7 V per cell and the 80% efficiency of a good cell, that is 16–18 kWh per kilogram — about a week's work from a small 100 W Water Turbines and Hydroelectric Power or Wind Turbines for a single kilogram. The chlorine that comes off (about 3 kg per kg of magnesium) is a valuable by-product (Chlorine and Bleach, Hydrochloric Acid), and a deadly danger if not captured.

Where to find it

Source Where How to recognise it
Seawater Any coast Bitter as well as salty: the bitterness is magnesium
Bittern The liquid left in salt pans after the common salt has crystallised (Salt) Oily-feeling, very bitter liquid that does not dry out in the sun; 30–60 g of magnesium per litre, twenty to forty times richer than seawater
Dolomite Thick grey to buff beds among limestones Fizzes only weakly in cold vinegar, strongly when powdered or warm. See Rocks and Minerals
Magnesite Veins and masses in serpentine and altered green rocks; some sedimentary beds White, dense, porcelain-like lumps that look like chalk but are harder and heavier; fizzes only in hot acid
Seashells and limestone For making the lime that precipitates magnesium Lime
Salt-lake crusts and potash beds Some dry lake beds and buried salt deposits Bitter, sticky salts that draw water from the air; carnallite (a potassium-magnesium chloride) is one

What you need

Item Amount Notes
Bittern or seawater 1 m³ of bittern, or about 30–50 m³ of seawater, for roughly 30–60 kg of magnesium Bittern from your salt works is the sensible start
Slaked lime About 3 kg per kg of magnesium From burnt shells, limestone, or better burnt dolomite, which brings its own magnesium (Lime)
Settling tanks Two or three, wood or masonry, 1–2 m³ With a tap 10 cm above the floor
Hydrochloric acid About 3 kg of pure acid per kg of magnesium Hydrochloric Acid; can be remade from the cell's chlorine
Iron pot Cast iron or welded steel, 30–60 cm across, with a lid The cathode and the cell body
Graphite rods 5–10 cm thick Anodes (The Electric Arc Furnace tells how to make carbon electrodes)
DC supply 6–8 V at 500–5,000 A Several large The Generators or a large rectified supply
Flux Potassium chloride and calcium chloride Makes the bath melt lower and protects the metal

Method 1: Magnesium compounds from bittern

This is achievable by any community with a salt works.

  1. Collect bittern. When you boil or sun-evaporate brine for salt, stop when salt crystals are coming out and the liquid has shrunk to about a thirtieth of the original seawater. Ladle off this thick, bitter bittern into clay jars. Do not throw it away.
  2. Epsom salt. Let bittern stand in shallow pans on cold nights. Long, clear, needle-shaped crystals of Epsom salt (magnesium sulfate) form when it cools below about 10 °C. Drain and rinse them with a little cold water. Dissolved and recrystallised once, they are pure enough to use as a laxative (an adult dose is about 10–15 g in a glass of water) or a foot soak. On farms, 20–40 kg per hectare cures the yellow-veined leaves of magnesium shortage (Understanding Soil).
  3. Magnesium hydroxide. Dilute bittern with three times its volume of fresh water. Stir in milk of lime — slaked lime mixed with water to the thickness of cream — slowly, until a drop of the clear liquid turns red cabbage juice green (Acids, Bases and Testing). A white, fluffy cloud forms and settles over several hours. Pour off the clear liquid, refill with fresh water, stir, settle again three times to wash out the salt.
  4. Use it wet as "milk of magnesia" (a gentle antacid and laxative — after boiling the water), or dry and burn it at a red heat to magnesia, a light white powder.
  5. Magnesia bricks. Magnesia from magnesite or from step 4, burned again at a white heat (1,600 °C and above, "dead-burned"), packs into bricks and furnace bottoms that resist basic slags far better than clay (Firebrick and Refractories, Steel in Quantity).
  6. Sorel cement. Mix lightly burned magnesia (burned at a dull red, not a white heat) with a strong magnesium chloride solution — about 2–3 parts magnesia to 1 part solution — into a stiff paste, with sawdust or sand as filler. It sets in hours to a hard, warm-feeling, polishable stone. It is good for indoor floors, grindstones and plaster, but it softens if kept wet, so do not use it outdoors.

Method 2: Magnesium metal by electrolysis (in outline)

1 Bittern + milk of lime; white flakes form 2 Settle, wash magnesium hydroxide sludge; pour off 3 Dissolve in hydrochloric acid: magnesium chloride 4 Boil down, dry slowly, in a stream of hydrogen chloride gas 5 Molten cell 700–750 °C; metal floats, chlorine rises chlorine from the cell is burned with hydrogen back into hydrochloric acid
Fig. 1 From seawater to metal. Lime throws magnesium hydroxide out of seawater or bittern; acid turns it into magnesium chloride; the chloride is dried and melted in an iron cell, where the current lifts magnesium to the surface and chlorine off the carbon anode.

This is the route the Dow Chemical Company used from 1941 to make most of the world's magnesium from seawater. Expect months of trial before a cell runs well.

  1. Precipitate. Make magnesium hydroxide as in Method 1, steps 3–4. For the metal it must be well washed: leftover calcium and sulfate foul the cell.
  2. Dissolve in acid. Stir the wet hydroxide into Hydrochloric Acid until no more dissolves. You get a clear magnesium chloride solution.
  3. Boil down. Evaporate in an iron or stoneware pan until a drop sets solid on a cold stone. Pour into trays and let it set to a white cake of hydrated magnesium chloride. It draws water from the air: keep it in sealed jars.
  4. Dry it. Heat the broken cake slowly in a closed iron retort, through which you blow dry hydrogen chloride gas, rising over a day from 100 °C to about 400 °C (dull red just showing in the dark). The gas stops the chloride turning into oxide as the water leaves. The Dow plants skipped the last step: they dried to about one and a half molecules of water and fed the hot, part-dry cake straight onto the molten bath, accepting some loss.
  5. Build the cell. A thick iron pot sits in a brick furnace that keeps it at about 700–750 °C (a cherry-red glow in a dim room). The pot itself is the cathode (−). Carbon anodes (+) hang down into the bath through a refractory lid, each inside a clay or firebrick hood that collects chlorine and carries it away through a pipe. The anodes must not touch the pot; keep them 5–10 cm apart.
  6. Make the bath. Melt a mixture of roughly 25% magnesium chloride, 15% calcium chloride and 60% sodium or potassium chloride. The added salts make the melt run at a lower temperature, conduct better and stay heavier than molten magnesium, so the metal floats.
  7. Run. Pass current at 6–7 V per cell. Bright, silvery beads of magnesium rise and gather in pools on the surface beside the cathode walls, outside the anode hoods. Feed fresh chloride as the bath is used up.
  8. Tap. Ladle the metal off with a perforated iron ladle every few hours and cast it into dry iron moulds, under a dusting of the same flux salt.

Another way: dolomite and ferrosilicon. Burned dolomite mixed with ferrosilicon (The Electric Arc Furnace) and heated to about 1,200 °C in a vacuum in a steel retort gives off magnesium vapour, which condenses as crystals at the cool end of the retort. This (the Pidgeon process, 1941) avoids chlorine but needs a good The Vacuum Pump and heat-resisting steel retorts (Alloy and Stainless Steels).

+ to the generator − (the pot is the cathode) Carbon anode in a firebrick hood that keeps chlorine away from the metal Chlorine out to an absorber or acid plant Magnesium floats ladle it off every few hours Molten salt bath magnesium, calcium and sodium chlorides, 700–750 °C Brick furnace keeps the pot cherry red Rising beads of metal
Fig. 2 The molten-salt cell in cross-section. The iron pot is the cathode; carbon anodes hang inside hoods that carry away the chlorine; magnesium rises and floats on the salt bath beside the pot wall.

Using magnesium

Use How Notes
Ductile iron Plunge magnesium (or a magnesium–ferrosilicon alloy, which reacts less violently) to the bottom of a ladle of molten iron under an iron bell Aim for 0.04–0.06% left in the iron. A violent, brilliant reaction: do it under a cover, everyone stood back
Light alloys About 9% aluminium and 1% zinc (cast); 3% aluminium and 1% zinc (wrought) Melt under a flux cover in an iron crucible, never clay (it reduces the clay). Cast into dry sand moulds
Aluminium alloys 0.5–5% magnesium in aluminium Harder, stronger, resists sea water (Aluminium)
Sacrificial anodes Cast blocks wired or bolted to steel Hulls, buried pipes (Pipes, Plumbing and Aqueducts), boilers and water tanks. Replace when half gone
Getter A tiny ribbon flashed by heat inside a vacuum tube after pumping Leaves a silvery mirror on the glass that soaks up gas (The Vacuum Tube, The Light Bulb)
Reducing other metals Molten magnesium with titanium or zirconium chloride in a sealed steel vessel full of argon The Kroll process (1940s) for Titanium — a long way ahead
Photographic light (historical) Burning ribbon gave the first indoor and underground photographs in the 1860s Dangerous; long since replaced by electric light (Photography)

Magnesium machines and files easily, but its chips catch fire. Keep tools sharp, never let swarf pile up, and sweep it into a metal bin with a lid.

How to tell it worked

  • Weight. A bar of magnesium feels startlingly light — lighter than aluminium of the same size.
  • Vinegar. A scrap dropped in vinegar fizzes steadily with hydrogen bubbles and dissolves; aluminium barely reacts with vinegar.
  • A thin shaving held in tongs in a candle flame flares with a blinding white light and leaves white ash (magnesia). Do this only with a shaving smaller than a fingernail clipping, outdoors, and do not look straight at it.
  • Epsom salt tastes intensely bitter, forms long needles, and does not crackle in a fire as common salt does.
  • Magnesia is so light and fluffy that a cupful weighs only a few tens of grams when freshly burned.

Note Troubleshooting. White sludge will not settle → too little lime, or the water is too cold and still. Add milk of lime until the test is alkaline, and leave it overnight. Cell gives no metal, only a grey sludge on the bottom → the chloride was not dry; it became magnesium oxide, which sinks and does nothing. Dry it better, or skim and remove the sludge. Metal forms as tiny beads that will not join and burn on the surface → bath too cold or too dirty. Raise the temperature toward 750 °C and add a little powdered fluorite (calcium fluoride, see Welding) to clean the beads. Chlorine leaks round the anodes → hoods cracked or not deep enough in the bath. Rebuild them deeper. Magnesium casting full of black specks and burnt surface → mould sand damp, or no flux cover. Use dry sand with a little sulfur or boric acid mixed in, and keep the melt covered.

Dangers

Danger Magnesium fire. Never use water. Burning magnesium reaches over 3,000 °C. Water on it is torn apart by the burning metal, giving off hydrogen that explodes and throws burning metal about. Carbon dioxide and most fire extinguishers make it worse; it even burns in nitrogen. Smother it with a deep pile of dry sand, dry salt or dry cast-iron filings, and let it burn out underneath. Keep a bin of dry sand and a shovel beside every place magnesium is melted, machined or stored. Fine powder and chips catch fire easily; a solid block is hard to ignite until it melts.

Danger Molten magnesium and water. Molten magnesium touching a damp mould, a wet ladle or a drop of rain reacts explosively. Every tool and mould must be bone-dry and preheated. Never cast in the rain.

Danger Chlorine. A magnesium cell gives off more than its own weight of chlorine gas. It burns the lungs and kills. Every anode must be hooded and piped to an absorber or a bleach plant (Chlorine and Bleach); work upwind with a wet cloth ready to cover your face.

  • Eyes. Burning magnesium gives off strong ultraviolet light that burns the eyes like a welding arc. Do not stare at it (Welding has the eye rules).
  • Hydrogen chloride and acid. Drying the chloride gives off choking acid fumes. Work outdoors.
  • Flash powders. Historically, magnesium powder mixed with oxidisers was used for photographic flash. These mixtures explode from a spark or a knock, killed and maimed photographers, and are not described in this book.
  • Too much Epsom salt causes severe diarrhoea and, in people with weak kidneys, can poison the heart. Keep to the dose.

What this unlocks

Ductile iron for strong, cheap castings (The Blast Furnace and Cast Iron); light alloys for engines and the Gliders and Aeroplanes; harder Aluminium alloys; getters for The Vacuum Tubes; magnesia Firebrick and Refractories for basic steelmaking (Steel in Quantity); sacrificial anodes for ships (Steamships) and pipes; and, much later, Titanium and Zircon and Zirconium.

How it was first done

Epsom salt was found in the bitter spring water at Epsom, England, in 1618, and became a famous purgative. The Scottish chemist Joseph Black showed in 1755 that "magnesia alba" was a separate earth from lime — work that also led him to discover carbon dioxide. Humphry Davy first separated a little impure magnesium by electrolysis in 1808, and Antoine Bussy made it in larger amounts in 1828–1831 by heating magnesium chloride with potassium. Robert Bunsen electrolysed molten magnesium chloride in 1852, the method still used. Magnesium ribbon lit the first photographs taken by artificial light in the 1860s. Germany produced magnesium industrially from the potash beds of Stassfurt from the 1880s and developed light "Elektron" alloys in the early 1900s. In 1941 Dow opened its seawater plant at Freeport, Texas; the same year, Lloyd Pidgeon in Canada developed the silicon-reduction process. Ductile iron was announced in 1948.