◆ Rebuild

Part 8 · Chemistry

Resins: Phenolic, Polyester and Epoxy

Cook phenol, urea or melamine with formaldehyde and you get syrups that, when heated, set once and for ever into hard, heat-proof plastic. This chapter covers the resin kettle they are cooked in; moulding powders pressed into switches, handles and melamine plates; paper and cloth laminates for circuit boards; urea glue for plywood; and, in outline, the polyester and epoxy resins of boats and two-part glues. It is honest about formaldehyde, phenol and hardeners, which poison and sensitise.

Difficulty
●●●●●
Time
An afternoon to cook a batch of resin once the chemicals are in hand; minutes per pressing; a week to set up a moulding shop
Steps from zero
22 prerequisites →

You need first

Composites: Fibreglass, Carbon Fibre and HoneycombCoal Tar Chemicals

This unlocks

—
The full path from nothing — 22 steps before this one
  1. Fire
  2. Stone Tools
  3. Finding and Preparing Clay
  4. Sulfur
  5. Simple Machines
  6. The Kiln
  7. Pottery
  8. Quarrying and Cutting Stone
  9. Lime
  10. Mining and Tunnelling
  11. Lye and Potash
  12. Fermentation
  13. Glass
  14. Saltpeter
  15. Distillation
  16. Coal and Coke
  17. Glass Fibre and Glass Wool
  18. Sulfuric Acid
  19. Coal Tar Chemicals
  20. Nitric Acid
  21. Early Plastics
  22. Composites: Fibreglass, Carbon Fibre and Honeycomb
  23. Resins: Phenolic, Polyester and Epoxy

Do them roughly in this order. See it on the tech tree →

Why it matters

Early Plastics introduced Bakelite in outline, and Composites: Fibreglass, Carbon Fibre and Honeycomb uses resins bought ready-made. This chapter is how to make them.

A thermosetting resin is a syrup or powder that, when heated or mixed with a hardener, links up into one giant molecule. Once set it cannot melt again; it only chars. That makes thermosets:

Phenolic and urea resins, from coal-tar phenol, wood-spirit formaldehyde and Urea, are the first a young chemical industry can make. Polyester and epoxy need more, and are given in outline.

How it works

Each formaldehyde molecule forms a bridge between two partner molecules. Phenol can take three bridges, urea four, melamine six, so the network grows in every direction until the whole mass is one molecule. You stop the reaction partway, while the resin is still liquid or meltable. Resin makers call the stages:

Stage State What you do with it
A-stage Syrup or brittle solid; dissolves in alcohol; melts Store it, mix it, soak paper in it
B-stage Rubbery when hot, no longer dissolves fully Moulding powder and laminate sheets are in this state
C-stage Fully set: hard, insoluble, cannot melt The finished part

Heat drives it. Phenolics cure in minutes at 150–170 °C; urea glues cold with an acid hardener. The reaction gives off water, which turns to steam in a hot mould, so these parts are pressed under great pressure. Polyester and epoxy set without giving off water, at room temperature and with no pressure, which suits hand-laid boats (Composites: Fibreglass, Carbon Fibre and Honeycomb) and glues.

The reaction makes heat. Phenol and formalin mixed with all their catalyst at once can heat themselves, boil, and throw hot resin out of the kettle. Every recipe below is built around controlling that heat.

Steam or hot oil inor cold water to cool Jacket3–5 cm gap Anchor stirrer40–100 turns/min,scrapes the walls Charging hole Enamelled potno bare iron or copper Motor thermometer resin Bottom valve5 cm or more: resin out fast out Condensercold water jacketwater outwater in Three-way valveback to pot (reflux)or down to receiver reflux Receiverwater takenoff the resinto vacuum vapour
Fig. 1 The resin kettle. A steel pot, enamelled inside, with a jacket for steam or hot oil and cold water, an anchor stirrer, a thermometer, and a condenser that can send vapour back into the pot (reflux) or off to a receiver (distilling off the water). A wide valve at the bottom lets the thick resin out quickly.

What you need

Item Notes See
Phenol Colourless crystals that turn pink; melts at 41 °C Coal Tar Chemicals
Formalin 37 % formaldehyde in water Methanol and Formaldehyde
Urea White crystals Urea
Ammonia water and caustic soda Alkaline catalysts Ammonia, Lye and Potash
Oxalic acid or hydrochloric acid Acid catalyst Oxalic Acid, Hydrochloric Acid
Wood flour Hardwood sawdust ground and sieved to pass 0.2 mm Sawmills and Lumber
Fillers: cotton linters or rag, paper pulp, mica, chalk Cotton, Paper
Pigment: lampblack, nigrosine dye, iron oxide Lampblack and Carbon Black, Pigments, Paints and Varnish
Zinc stearate or stearic acid Mould release, mixed into the powder Soap
Resin kettle, hot press and steel moulds Below Presses, Punches and Dies

Where to find it

Every chemical here is made in another chapter. The raw materials are coal (phenol, lampblack), hardwood (wood spirit, wood flour), cotton, and mica, the glittering mineral that splits into thin flexible sheets, found in granite and pegmatite (Rocks and Minerals).

The resin kettle

A resin kettle is pot, stirrer, heater, cooler and condenser in one.

Workshop size: 20–100 litres.

  1. Pot. Steel, about as deep as it is wide, with a dished bottom. Line the inside with vitreous enamel (Enamel on Metal) or make it of stainless steel or nickel. Bare iron or copper turns phenolic resins dark red and spoils urea and melamine resins. A glass-lined pot is best.
  2. Jacket. A second shell around the lower two-thirds, 3–5 cm away, welded or riveted on (Pressure Vessels and Valves, Welding). Run steam in for heating to about 120 °C, or hot oil to 180 °C, and cold water through it to cool fast. Never heat a resin kettle over an open fire alone: you cannot stop the heat in a hurry.
  3. Lid with: a central anchor stirrer (a U-shaped paddle that scrapes close to the walls, 40–100 turns a minute), a thermometer pocket reaching into the liquid, a charging hole with a cover, and a vapour pipe.
  4. Condenser on the vapour pipe: a coil in a water tank or a tube-in-tube (Distillation). A three-way valve sends the condensate either back into the pot (reflux, which holds the boiling liquid at 100 °C and soaks up the reaction heat) or into a receiver (distilling off water to thicken the resin).
  5. Vacuum connection on the receiver, so water can be taken off below 100 °C (The Vacuum Pump).
  6. Bottom valve, at least 5 cm wide. A resin that starts to gel must come out in minutes, not an hour.

Laboratory size: a 2-litre flask with stirrer, thermometer and reflux condenser in a water or oil bath (Laboratory Glassware).

Good and bad kettles. A good one holds temperature within 2–3 °C, cools from boiling to 60 °C in under 15 minutes, and has no dead corners. If you have to chisel set resin out of the bottom, the stirrer does not reach and the valve is too small.

Phenolic moulding

Making novolac resin

Novolac, made with less formaldehyde than phenol and an acid catalyst, melts but will not set until a hardener is added, so it keeps. It is the base of moulding powder.

For a 10-litre kettle:

  1. Melt 4.7 kg of phenol (50 moles) in the kettle at 50–60 °C.
  2. Add 3.3 kg of formalin (37 %; that is 0.8 mole of formaldehyde for every mole of phenol) and 50 g of oxalic acid dissolved in a little hot water.
  3. Heat slowly to boiling, about 100 °C, with the condenser on reflux. Watch the thermometer. When it starts to rise on its own, shut off the heat; let the reflux carry the heat away.
  4. Reflux for 2–3 hours. The mixture turns milky, then separates into a heavy, honey-coloured resin layer and watery top.
  5. Switch the condenser to the receiver. Distil off the water, first at ordinary pressure, then under vacuum, while the temperature climbs to 140–160 °C.
  6. Test a drop: pulled out on a cold steel plate, it should set to a brittle, glassy solid that snaps cleanly.
  7. Run it out of the bottom valve into shallow trays. Break it into lumps when cold. Yield about 5 kg.

Hexamine, the hardener

Hexamine is a white crystalline powder made by mixing formalin with ammonia water (about 6 parts of formaldehyde to 4 of ammonia, by molecules) and evaporating it gently to dryness below 60 °C (Ammonia). When heated in the mould, it gives off formaldehyde and ammonia, which link the novolac into a solid.

Moulding powder

Press ram100–200 tonnes for a 25 cm plate Heated platensteam or electric, 150–165 °C Top half (force)hardened, polished steel The platewall 2–2.5 mm Flashthin fin, trimmed off Foot ring Guide pins Bottom half (cavity) dinner plate: 20–25 cm across foot ring 8–12 cm across Finished plate150–200 g of powder;2–3 minutes in the press
Fig. 2 A compression mould for a melamine or phenolic plate. The two hardened steel halves are heated to 150–170 °C. A weighed charge of powder goes in the open cavity; the top half comes down under heavy pressure, the powder melts, flows to fill the space, and sets. Extra resin squeezes out as a thin flash at the parting line.

A general-purpose black phenolic powder, by weight:

Ingredient Parts
Novolac resin 100
Hexamine 12
Wood flour 100
Lime or magnesia 2
Zinc stearate 2
Nigrosine or lampblack 3

For heat- and spark-proof electrical parts, replace half the wood flour with ground mica; for tough gear blanks, use cotton rag chopped to 5 mm.

  1. Grind resin and hexamine together to pass a 0.5 mm sieve. Keep them dry.
  2. Mix everything in a tumbling drum for half an hour.
  3. Roll the mix between two steel rolls heated to 90–110 °C, one slightly faster than the other, for 3–5 minutes, until it forms a sheet. This melts the resin through the wood flour and moves it just into the B-stage. Too long and it sets on the rolls.
  4. Cool the sheet, break it, and grind it to a powder that passes a 2 mm sieve.

Pressing a moulding

  1. Mould: two halves of hardened, polished tool steel that fit with a small gap at the edge, about 0.1 mm (Presses, Punches and Dies, Forge Shops and Heat Treatment). Allow for the part to shrink 0.6–1 % as it cools. Chrome-plating the cavity helps release (Electroplating).
  2. Heat the mould to 150–170 °C: a pinch of sulfur on it should melt and turn dark red-brown.
  3. Charge: weigh enough powder for the part plus about 5 %. Preheating the powder to 80–100 °C halves the cure time.
  4. Press at 15–30 MPa on the area of the part (150–300 kg on each square centimetre). A 10 cm part needs a press of about 25 tonnes (Hydraulic Presses and Rams).
  5. Breathe: after 10–20 seconds, open the mould a crack for a second to let out steam and gas, then close again.
  6. Cure: about 40–60 seconds for each millimetre of the thickest wall.
  7. Open, lift the part out hot, and snap or file off the flash, the thin fin at the parting line.

Sizes. Walls 2–6 mm; ribs no thicker than the wall; holes at least one diameter from an edge.

Good and bad. A good moulding is glossy, evenly coloured, rings when tapped, and breaks dense and even. Blisters: too little breathing or cure. Dull, rough patches: damp powder or a cold mould. Soft centre: too short a cure. Cracks: the part stuck; add stearate or polish the mould.

Phenolic laminate

Phenolic laminate is paper or cotton cloth bonded with phenolic resin into a hard board: insulating panels, silent gears and bearings, and the base of circuit boards (Building Circuits: Boards, Connectors and Cables).

Paperor cotton 1. Resol varnishresin in alcohol 2. Dry120–140 °C, minutes:B-stage, dry to touch cut to size 3. Hot press 140–160 °C, 7–10 MPa, 1 hour; cool under pressure; polished steel plates between packs;8 sheets of paper per mm of board
Fig. 3 Making phenolic laminate. Paper or cotton is drawn through resol varnish, dried in a warm oven until it is dry to the touch, cut, and stacked between polished steel plates in a heated press.
  1. Resol varnish. In the kettle, heat 1 part phenol with 1.5 parts formalin (by moles, about 1 : 1.5) and 2 % ammonia water (on the phenol) at 70–80 °C, not boiling, for 1–2 hours, until it clouds and a resin layer forms. Distil off water under vacuum below 70 °C until it is a thick syrup, then thin it with an equal weight of alcohol (Ether, Acetone and Solvents). This is a resol: it needs no hardener and sets by heat alone, so keep it cool and use it within weeks.
  2. Impregnate. Draw sheets of kraft paper or cotton cloth through the varnish and hang them to drain.
  3. Dry in an oven at 120–140 °C for a few minutes, until the sheets are dry to the touch but a sheet held to a hot iron still goes glossy. They are now B-stage.
  4. Stack the sheets between polished steel plates: about 8 sheets of paper for each millimetre of board.
  5. Press in a heated platen press at 140–160 °C and 7–10 MPa for 1 hour, then cool under pressure before opening.

Good and bad. Good board is hard, brown and translucent at the edges. It does not swell after an hour in boiling water and does not spark through under a The Induction Coil at a few thousand volts. Pale, soft layers mean the resin was too thin; splitting layers mean the sheets were over-dried.

Decorative laminate (worktops): a top sheet of printed paper soaked in melamine resin (below) over a phenolic paper core, pressed together.

Urea-formaldehyde glue

Pale, cheap, strong and set cold: the glue of indoor plywood, chipboard and furniture (Plywood, Veneer and Boards, Glues and Adhesives). Outdoors, use phenolic resin.

  1. In the kettle, put 2 kg of formalin (37 %) and bring it to pH 7.5–8 with a little caustic soda (pH, Indicators and Buffers).
  2. Add 0.75 kg of urea (about 1 urea to 2 formaldehyde, by molecules). Heat to 90 °C for 30 minutes.
  3. Add a few drops of formic or acetic acid to bring it to pH 5. Hold at 90–95 °C. Every few minutes drop a little into cold water. When the drop turns cloudy white and no longer dissolves, it is ready. This takes 20–60 minutes.
  4. At once bring it back to pH 7.5–8 with caustic soda and cool. Stir in 0.25 kg more urea: this soaks up spare formaldehyde and cuts the smell.
  5. Distil off water under vacuum to a syrup of about 60–65 % solids, like thin honey. Keep it cool; it lasts 2–3 months.

Using it. To 100 parts of syrup stir in 10–20 parts of wheat flour (a filler that stops it soaking too far into the wood) and 1–2 parts of ammonium chloride dissolved in a little water as the hardener. It stays usable for 2–4 hours. Spread thinly on both faces, assemble, and clamp at 0.5–1 MPa for 8–12 hours at 20 °C, or press for about 1 minute per millimetre of wood between plates at 100–110 °C.

Good and bad: glue two strips of hardwood with a 25 mm overlap and break them after a day. The wood should tear, not the glue line. A glue line that peels clean was starved (too thin), the hardener was old, or the wood was oily or wet.

Melamine plate

Melamine is a white crystalline powder made by heating urea to about 400 °C under ammonia pressure in an alloy steel vessel, or from dicyandiamide made from calcium cyanamide (Calcium Carbide and Acetylene, Urea). Both are works processes, described in Calcium Cyanamide, Dicyandiamide and Melamine. With formaldehyde it makes the hardest, most scratch-proof and heat-resistant of the pale resins.

Resin. Stir 1 part of melamine into 2.5 parts of formalin by molecules (about 1 kg of melamine to 1.6 kg of formalin), at pH 8.5–9.5 with a little caustic soda, and heat to 85–90 °C. The melamine dissolves. Hold until a drop clouds in cold water, usually 30–60 minutes, then cool.

Moulding powder.

  1. Knead the warm syrup into pure white cellulose: bleached cotton linters or bleached paper pulp (Laundry and Bleaching Cloth), about 35 parts cellulose to 65 parts resin solids.
  2. Dry it at 80–90 °C to a crumbly cake, then grind it fine with 1 % zinc stearate, 0.2 % of a mild acid catalyst such as phthalic anhydride, and a white or pastel pigment (titanium white, Titanium; or food-safe mineral colours).

Pressing a plate.

Dimension Typical
Diameter 20–25 cm (dinner); 15–18 cm (side)
Wall 2–2.5 mm
Foot ring 8–12 cm across, 4–5 mm high
Rim radius at least 5 mm (sharp corners crack)
Powder per dinner plate about 150–200 g
  1. Heat the steel mould to 150–165 °C.
  2. Pour in the weighed powder, spread evenly. For a decorated plate, press it once for 30 seconds, open, lay a printed paper foil soaked in melamine resin on the face, and close again.
  3. Press at 20–40 MPa on the plate area, which for a 25 cm plate means 100–200 tonnes. Breathe once after 15 seconds.
  4. Cure 2–3 minutes. Lift out hot, trim the flash, and buff the edge.

Good and bad. A good plate is glossy, even and rings when flicked. It does not stain from tea after an hour or lose its shine after 30 minutes in boiling water. Blisters, a dull or crazed surface, or a smell of formaldehyde when hot mean undercure. Throw away plates that are cracked, deeply scratched or crazed: food lodges in them.

Warning Melamine plates are for serving, not cooking. Do not use them in an oven or microwave, or for food hotter than about 70 °C, especially acid food. Heat slowly breaks the resin and releases formaldehyde and melamine into the food. Never add melamine to food or animal feed: in 2008 milk powder deliberately spiked with it sickened about 300,000 Chinese babies and killed six.

Polyester and epoxy, in outline

Both need chemicals from a mature organic works (Organic Synthesis and Fine Chemicals, Petroleum and Refining).

Unsaturated polyester. In a kettle under a blanket of carbon dioxide, cook 1 mole of phthalic anhydride (from naphthalene, Coal Tar Chemicals), 1 mole of maleic anhydride and about 2.2 moles of propylene glycol at 190–210 °C for 8–14 hours, distilling off water, until a titration shows the acid nearly used up. Cool to about 100 °C and thin with styrene to about 65 % resin, with a pinch of hydroquinone to stop it setting in the drum. It is cured with peroxide and cobalt as in Composites: Fibreglass, Carbon Fibre and Honeycomb.

A simpler cousin, alkyd resin, from phthalic anhydride, glycerine (Soap) and linseed oil, makes tough enamel paints (Pigments, Paints and Varnish).

Epoxy needs bisphenol A, from phenol and acetone with strong hydrochloric acid (Ether, Acetone and Solvents), and epichlorohydrin, from glycerine, hydrogen chloride and caustic soda. Stirred together with caustic soda at 60–100 °C, they give a clear, thick liquid epoxy resin. The usual hardeners are amines made from ammonia, or "polyamides" made from amines and fatty acids, which mix 1 : 1 and are gentler on the skin.

Epoxy glue

A two-part glue: resin in one tube, hardener in the other.

Making it. Fill one tube with liquid epoxy resin. Fill the other with an equal volume of polyamide hardener. For a gap-filling glue, stir up to an equal volume of fine chalk or silica flour into each. Fill soft metal tubes (Tin and Pewter) or a double syringe. Label them A and B and say the ratio.

Using it.

  1. Clean and roughen both surfaces: sand, file, or scour; wipe off grease with alcohol or acetone.
  2. Measure exactly: equal lengths from each tube, or the weights the maker states. Wrong ratios never cure fully.
  3. Mix for a full minute on a scrap of card until the colour is perfectly even.
  4. Spread thinly on both faces, press together, and hold lightly. Do not squeeze it all out.
  5. Leave 24 hours at 20 °C, or 1–2 hours at 60–70 °C. Below 10 °C it barely cures.

Good and bad: a good joint in steel lap strips (25 mm overlap) takes a hard blow with a hammer. A drop of left-over glue on the card should be hard as horn the next day. Tacky glue means wrong ratio or poor mixing; a white bloom means it cured in damp cold air.

How to tell it worked

  • Gel time: put a pea of resin and hardener (or moulding powder) on a hot plate at 150 °C and stroke it with a spatula. Novolac powder should go stringy then rubbery in 60–120 seconds. Far quicker and it will set before the mould fills; far slower and parts will blister.
  • Cure: wipe a part with acetone for a minute. A fully cured phenolic or melamine part stays glossy; an undercured one goes dull or tacky.
  • Boiling water: 30 minutes in boiling water should not swell, whiten or soften a good part or glue line.

Note Troubleshooting. Resin boiled over or set solid in the kettle → catalyst added too fast or too much, or heat left on after the reaction took off. Add catalyst in portions and cut the heat once the thermometer starts climbing alone. Novolac stays sticky when cold → not enough water taken off. Distil it further. Melamine plates crack round the foot → wall too thick there, or sharp inside corners. Urea glue weak → too old, too little hardener, wood too wet (over about 12 %) or too dry and porous.

Dangers

Danger Phenol passes straight through skin and numbs as it burns. Strong phenol splashed over a large area, such as a whole arm, has killed people within hours (Coal Tar Chemicals). Wear rubber gloves, apron and goggles. Wash any splash at once with plenty of water for at least 15 minutes; wiping with vegetable oil or glycerine first lifts it faster (Early Plastics, Emergencies).

Danger Runaway reactions. The phenol–formaldehyde reaction can heat itself past boiling in minutes. Have the cooling water ready before adding catalyst, keep the reflux condenser open, never seal a hot kettle, and stand back from the charging hole.

  • Formaldehyde stings eyes and lungs, causes asthma and skin allergy, and causes cancer with long exposure (Methanol and Formaldehyde). Work with ventilation; ventilate the press shop too, since hot mouldings give off fumes.
  • Hexamine dust is flammable and causes skin allergy.
  • Epoxy hardeners burn skin, and epoxy resin causes allergy that grows with every exposure until the smell alone brings a rash. Never let either touch skin. Epichlorohydrin is very poisonous and causes cancer: a works chemical only.
  • Styrene is flammable and harmful to breathe; peroxide catalysts must never be mixed directly with cobalt accelerator (Composites: Fibreglass, Carbon Fibre and Honeycomb).
  • Moulding powder and wood-flour dust can explode in a cloud. Keep the shop swept.

What this unlocks

Safe switches, sockets and lamp holders (Insulators, Cables and Electrical Fittings, Wiring and Electrical Safety); circuit boards (Building Circuits: Boards, Connectors and Cables); weatherproof plywood and chipboard (Plywood, Veneer and Boards); washable tableware and worktops; brake linings and grinding wheels bonded with phenolic resin (Abrasives and Grinding Stones); foundry sand cores (Metal Casting); and the resins for fibreglass and carbon-fibre (Composites: Fibreglass, Carbon Fibre and Honeycomb).

How it was first done

Adolf von Baeyer noticed in 1872 that phenol and aldehydes gave a sticky resin. Leo Baekeland in Yonkers, New York, learned to control it with heat and pressure and patented Bakelite in 1907–09. Urea-formaldehyde was patented by Hanns John in Prague in 1918, and British Cyanides sold white "Beetle" urea mouldings from 1925. Melamine resin came from American Cyanamid and Ciba in the 1930s, and melamine tableware became common after the Second World War. Carleton Ellis patented unsaturated polyesters in 1936, and Pierre Castan in Switzerland and Sylvan Greenlee in the United States developed epoxy resins in the late 1930s and 1940s.

Source: content/entries/chemistry/thermosetting-resins.md