◆ Rebuild

Part 3 · Metals

Palladium, Rhodium and Iridium

Crude platinum carries five sister metals, each with a job nothing else does as well. Palladium soaks up hydrogen and makes catalysts, dental alloys and white gold; rhodium gives thermocouples that read furnaces to 1,700 °C and a bright plating that never tarnishes; iridium gives crucibles for melts hotter than platinum can stand and the hard tips of fountain pens. How to separate them from platinum residues in outline, how to make each object, and why osmium must be treated as a poison gas.

Difficulty
●●●●●
Time
Weeks to months to gather residues worth working; days for each separation; a day to make a thermocouple; an afternoon to tip and grind a pen nib once the grains are sorted
Steps from zero
25 prerequisites →

You need first

Platinum and the Platinum Metals

This unlocks

—
The full path from nothing — 25 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Lime
  14. Salt
  15. Lye and Potash
  16. Glass
  17. Bellows
  18. Saltpeter
  19. Copper Smelting
  20. Lead
  21. Sulfuric Acid
  22. Gold and Silver
  23. Nitric Acid
  24. Hydrochloric Acid
  25. Platinum and the Platinum Metals
  26. Palladium, Rhodium and Iridium

Do them roughly in this order. See it on the tech tree →

Why it matters

The Platinum and the Platinum Metals chapter keeps every residue and every liquor from refining. This chapter is what to do with them. Together they hold palladium, rhodium, iridium, osmium and ruthenium, a few per cent of the crude metal, and each does one job better than anything else:

  • Palladium drinks up hydrogen and lets only hydrogen through it. It makes the catalysts that add hydrogen to oils and medicines, filters that give the purest hydrogen, long-lasting relay contacts, white gold and dental crowns.
  • Rhodium alloyed with platinum gives thermocouples that read kilns, glass tanks and steel furnaces to 1,700 °C (Thermocouples and Thermoelectricity), the long-lived gauzes of the nitric acid works, and a white, mirror-bright plating that never tarnishes.
  • Iridium is the most corrosion-proof metal known. It stiffens platinum, makes crucibles that hold melts above 2,000 °C, and with osmium makes the hard tips that let a gold pen nib write for a lifetime.
  • Osmium and ruthenium are mostly a danger to be managed (below).

A community will have grams of these, not kilograms. Spend them where nothing else will do.

How it works

Metal Times as heavy as water Melts at What dissolves it Colour of its chloride solution
Platinum 21.4 1,768 °C Aqua regia Orange-yellow
Palladium 12.0 1,555 °C Hot nitric acid alone; aqua regia Red-brown
Rhodium 12.4 1,964 °C Nothing, as solid metal; fused bisulfate takes the powder Rose-red
Iridium 22.6 2,446 °C Nothing; chlorine or fused alkali at red heat Dark red-brown to black
Osmium 22.6 about 3,030 °C Oxidisers turn it into a volatile poison
Ruthenium 12.4 2,334 °C Fused alkali with oxidiser; also volatile oxide

Separating them depends on three differences: palladium dissolves in nitric acid and forms a yellow salt with ammonia; rhodium alone dissolves in fused bisulfate; iridium does not dissolve in aqua regia at all, so it stays with osmium in the insoluble residue. Everything is done on grams, in porcelain and glass, slowly, with every liquid kept and labelled.

What you need

Item Use See
Platinum residues, osmiridium, anode slime Raw material Platinum and the Platinum Metals, Nickel and Cobalt
Nitric Acid, Hydrochloric Acid, Ammonia water, sal ammoniac Dissolving and precipitating
Potassium bisulfate (from potash and Sulfuric Acid) Rhodium fusion Lye and Potash
Porcelain dishes, crucibles, glass funnels, filter paper All steps Laboratory Glassware
Oxy-hydrogen or oxy-gas blowpipe, lime blocks Melting Hydrogen, Oxygen and Gases, Very-High-Temperature Furnaces
Hydrogen supply Reducing sponges Hydrogen, Oxygen and Gases
Draw plates, small rolling mill Wire and sheet Iron and Brass Wire, Sheet Metal and Rolling
A strong fume draught or open-air bench Everything Ventilation and Air Conditioning

Where to find it

  • Platinum residues. The liquor poured off the yellow platinum salt, the black mud that iron strips throw down from it, and the insoluble black sand and flakes left after aqua regia (Platinum and the Platinum Metals).
  • Osmiridium (also called iridosmine): tiny, bright, tin-white, flat six-sided flakes in platinum and some gold placers, too hard for a steel needle to scratch, not touched by any acid. See the materials glossary.
  • Anode slime from refining nickel and copper made from sulfide ores such as pentlandite (Nickel and Cobalt). Some nickel ores carry more palladium than platinum.
  • Scrap: thermocouple wire, gauzes, contacts, dental gold.

Separating them (in outline)

Crude platinum grains Insoluble black sand and osmiridium grains Orange-red solution PLATINUM yellow salt, sponge Mother liquor + iron gives a black mud PALLADIUM yellow ammine salt Rose-red remainder thrown down on iron RHODIUM dissolves in the melt Undissolved: iridium, some platinum PEN TIPS osmiridium grains used whole Osmium leaves as a gas: TRAP IT in caustic soda Iridium solution + sal ammoniac: dark salt IRIDIUM sponge, pressed and forged aqua regia sal ammoniac mother liquor aqua regia, ammonia, then acid fuse with bisulfate and leach simplest use salt + chlorine, red heat dissolve what is left
Fig. 1 The separation of the platinum metals in outline. Crude platinum dissolves in aqua regia, leaving osmiridium. Sal ammoniac throws down platinum. Iron throws the remaining metals out of the liquor as a black mud, which is redissolved; ammonia and then hydrochloric acid give yellow palladium salt. What remains is fused with bisulfate, which dissolves rhodium and leaves iridium. Osmiridium is attacked by chlorine with salt at red heat, releasing osmium, which must be trapped, and leaving iridium in solution, which sal ammoniac throws down as a dark salt.

Palladium

  1. Collect the black mud from the platinum liquors. Dissolve it in warm aqua regia outdoors, drive off the nitric acid with repeated additions of hydrochloric acid, and dilute (Platinum and the Platinum Metals, Step 1).
  2. Remove the last platinum with sal ammoniac as before; filter off the yellow salt and return it to the platinum stock.
  3. Add ammonia water until the liquid smells strongly of it. Iron falls as brown rust and is filtered off; copper turns the liquid deep blue; palladium dissolves as a nearly colourless ammonia compound.
  4. Add hydrochloric acid slowly to the clear filtrate until it is acid. A yellow crystalline powder falls: palladium diammine chloride, the "yellow palladium salt". Copper stays dissolved.
  5. Repeat steps 3–4 twice, dissolving the salt in ammonia and throwing it down with acid, until the ammonia solution is no longer blue.
  6. Ignite the dry salt gently in a porcelain crucible outdoors, then heat the grey sponge to a bright red in a stream of hydrogen, or under a layer of charcoal, and let it cool there. Palladium heated in air tarnishes blue-violet with oxide at a dull red, and loses it again at a bright red.
  7. Melt the sponge on a lime block with an oxy-hydrogen flame, or press and sinter it like platinum. Palladium is soft and malleable; it forges, rolls and draws like gold.

Rhodium

  1. What is left after palladium is removed still holds rhodium, colouring the liquid rose-red, with some iridium. Throw down all the metals as a black powder with clean iron or zinc, wash, and dry it.
  2. Fuse the powder with five to ten times its weight of potassium bisulfate in a porcelain crucible at a dull red heat for an hour. Rhodium turns into a soluble sulfate; iridium, platinum and osmiridium do not.
  3. Leach the cold melt with hot water: a yellow to rose solution. Filter. Repeat the fusion on the residue until the leach is colourless.
  4. Precipitate rhodium hydroxide with caustic potash, wash, dissolve in hydrochloric acid, and reduce it to rhodium black by warming with formic acid, or with zinc, and wash with acid.
  5. Ignite in hydrogen to grey rhodium sponge, used as it is for alloying or plating.

Iridium (and osmium)

The simplest use of iridium needs no separation at all: osmiridium grains make pen tips as they are (below). To get iridium metal:

  1. Open up the insoluble residue and osmiridium. The classic way is to mix it with twice its weight of common salt and heat it red-hot in a tube of porcelain or glass through which chlorine gas passes (Chlorine and Bleach). Iridium becomes a soluble double chloride. Osmium comes off as its tetroxide, a deadly vapour (see Dangers), and must be led into a trap of caustic soda solution with a little alcohol, which holds it. Another route is fusion with sodium peroxide in an iron or nickel crucible, which also frees osmium.
  2. Dissolve the product in water with a little hydrochloric acid, pass chlorine or add a little nitric acid to make sure the iridium is fully oxidised, and add sal ammoniac: a dark red-black crystalline salt falls, ammonium chloroiridate.
  3. Ignite it and heat the sponge in hydrogen. Iridium sponge is pressed and sintered at 1,500 °C or more and forged only white-hot; cold, it is brittle.

Warning Do not attempt the iridium route without a strong draught that carries fumes away from people, an osmium trap, and chlorine handled outdoors. For most needs, buy, trade for or salvage iridium already separated, or use osmiridium grains whole.

The rhodium thermocouple

Platinum against platinum–10 % rhodium (type S) is made in Platinum and the Platinum Metals. Two more rhodium couples matter:

Couple Wires Good to Output at 1,000 °C Notes
Type R Pt–13 % Rh against Pt 1,450–1,500 °C 10.5 mV Like S, slightly stronger signal
Type B Pt–30 % Rh against Pt–6 % Rh 1,700 °C (1,800 °C briefly) 4.8 mV Both wires alloyed: lasts longer, drifts less, very low output below 100 °C

Type B readings, cold junction at 0 °C: 600 °C, 1.79 mV; 1,000 °C, 4.83 mV; 1,200 °C, 6.79 mV; 1,400 °C, 8.96 mV; 1,600 °C, 11.26 mV; 1,800 °C, 13.59 mV. Because it gives almost nothing below about 50 °C, its cold junction can sit at room temperature with an error of less than a degree, and plain copper wires serve as its leads.

Closed-end sheath gas-tight alumina, 8–12 mm Twin-bore tube purest alumina end view Pt–30 % Rh (positive, stiffer) Pt–6 % Rh (negative) Welded bead the hot junction Terminal head Millivoltmeter copper leads are enough for type B Calibrating by the wire bridge a 5 mm piece of pure gold (1,064 °C) or palladium (1,555 °C) joins the wires; when it melts the circuit breaks: read the last value
Fig. 2 A rhodium thermocouple taken apart. Two thin platinum–rhodium wires, welded into a bead at the hot end, run through a twin-bore tube of pure alumina inside a closed alumina sheath, to a terminal head where copper leads carry the millivolts to the meter. Beside it, how the wire bridge calibration works: a short piece of gold or palladium wire joins the two wires and breaks the circuit when it melts.

Making it

  1. Alloy. Weigh platinum and rhodium sponge exactly (for type B: 70 g Pt with 30 g Rh, and 94 g Pt with 6 g Rh). Press each mix, sinter it white-hot, and melt it on a lime block in the oxy-hydrogen flame, turning and remelting the bead three or four times so it is even (Very-High-Temperature Furnaces).
  2. Forge, roll and draw to 0.5 mm (0.35 mm for small furnaces), annealing bright yellow-hot in a clean flame every few passes. The 30 % alloy is much harder than platinum; anneal it often. A 1 m pair of 0.5 mm wires weighs about 8 g.
  3. Mark the wires: the stiffer wire is the more rhodium-rich (positive) one. Tie a thread or cut a nick.
  4. Weld the junction: twist 3 mm together and fuse into a small bead in an oxy-gas flame, or with a carbon arc.
  5. Insulate with a twin-bore tube of the purest alumina you can make (Alum and Alumina, Firebrick and Refractories), inside a closed-end, gas-tight alumina sheath 8–12 mm across. Silica, iron, carbon, phosphorus, sulfur and metal vapours all poison platinum wire at high heat; the sheath keeps them out. Never use a rhodium couple bare in a smoky or reducing flame.
  6. Head. At the cool end, a small porcelain block with two brass screw terminals in a cast metal head. For types R and S, use compensating leads of copper and copper–nickel; for type B, plain copper.
  7. Anneal the finished couple by passing current through it in air until it glows bright yellow for a few minutes.

Calibrating and judging it

Wire bridge method. Join the two wires with a 5 mm piece of pure gold wire (melts at 1,064 °C) or palladium wire (1,555 °C) and heat the couple slowly in the furnace. At the melting point the circuit breaks; the last reading is the calibration point. Check a type B in a platinum-melting test (1,768 °C) only if you must; it shortens its life.

Good versus bad. A good couple reads the gold point within 2 °C and drifts less than a few degrees a year in clean service. Wire that has gone brittle, grainy or discoloured near the hot end has been poisoned; cut that part off and re-weld, or remelt it. A sudden jump to zero is a broken wire; a slow low reading, contamination or a cold junction gone warm (types R and S).

Rhodium plating

Rhodium plate is white, harder than steel, and does not tarnish in any air. A thickness of 0.1–0.5 µm protects silver jewellery, searchlight and instrument mirrors, and sliding electrical contacts (Electroplating, Mirrors).

  • Bath: dissolve washed rhodium hydroxide in dilute sulfuric acid to give 2 g of rhodium per litre with about 20–40 ml of strong sulfuric acid per litre.
  • Run at 40–50 °C and 1–2 A per dm², with a platinum anode (anything else dissolves into the bath). The work is first plated with nickel or silver and must be spotless.
  • Time: a few minutes gives a bright, white coat.

A good coat is mirror-bright, bluish-white, and survives rubbing with a cloth and a drop of nitric acid unmarked. Grey or dark plate means too high a current or a dirty bath.

The iridium pen tip

A gold nib (Pens, Nibs and Writing Instruments) is soft. Within a few months of daily writing its point wears into a flat, scratchy wedge. A grain of osmiridium on the point outlasts its owner. Steel nibs rust in fountain pens; this is the answer.

1 Blank 14-carat gold, point blunt and not slit 2 Solder the grain borax and gold solder, fine flame from behind 3 Grind it round copper wheel with diamond powder 4 Cut the slit thin copper disc with diamond dust 5 Finished tines level, touching, polished smooth breather hole grain 0.6–1 mm
Fig. 3 Tipping a gold nib with osmiridium. 1: the nib blank, its point left blunt. 2: a sorted grain set on the point with borax and a chip of gold solder, heated with a fine blowpipe flame until the solder flows round it. 3: the grain ground round on a copper wheel charged with diamond powder. 4: the slit cut through the tip with a thin copper disc and diamond dust. 5: the finished point, tines level and touching, polished smooth.
  1. Sort the grains. Under a strong lens, pick bright, compact grains 0.6–1.0 mm across, without cracks. Flat flakes can be stood on edge. Keep the rest for later.
  2. Prepare the nib. Cut and form the nib blank of 14-carat gold (58 % gold, the rest silver and copper) 0.25–0.3 mm thick, as in Pens, Nibs and Writing Instruments, but leave the point blunt and unslit. File a tiny seat in the end of the point to hold the grain.
  3. Solder the grain. Wet the point with borax paste (Borax and Boric Acid), set the grain in the seat with fine tweezers, add a chip of hard gold solder, and play a small, sharp blowpipe flame from behind the nib until the solder flows round the grain and grips it (Soldering and Brazing). The grain does not melt. Pickle in warm dilute acid and wash.
  4. Grind the tip round. Osmiridium is far too hard for files. Use a small copper or soft iron wheel turning at a few hundred rpm, charged with diamond powder in oil (Industrial Diamond and Hard Abrasives), or failing that the finest corundum (Abrasives and Grinding Stones). Grind the grain into a smooth ball blending into the gold.
  5. Slit it. Cut the slit through the tip with a thin copper disc, 0.1–0.15 mm, charged with diamond dust, then continue the slit along the gold to the breather hole with a fine saw. Close the tines so they touch at the tip.
  6. Shape the writing face. On a slowly turning lap or by hand on a fine stone, grind the underside flat at the writing angle (about 45° to the paper): about 0.3–0.4 mm wide for a fine point, 0.5–0.6 mm for a medium.
  7. Polish on leather or fine paper charged with diamond paste, writing figure-eights, until it glides.

Good versus bad. Under a lens, a good tip has both halves at exactly the same height, the slit centred, edges rounded, and no gap or overlap. It writes smoothly in every direction with no scratch, and keeps doing so after a year. A grain that rocks or a black line of solder showing round it will fall out; resolder it. A sharp edge means more polishing.

Modern tips are tiny balls of a melted ruthenium–osmium–iridium–tungsten alloy welded on electrically; they work the same way.

The iridium crucible

Platinum softens above about 1,600 °C. Iridium holds its shape to over 2,200 °C, and molten oxides do not wet it. Crucibles of it are used to grow single crystals of laser and gem materials by slowly pulling a seed from the melt (Synthetic Gems, Lasers).

  • Size: typically 50 mm across and tall, walls 1.5–2 mm, weighing about 400–450 g (it is 22.6 times as heavy as water).
  • Making it (outline): pressed and sintered powder, forged and rolled white-hot (cold, it cracks), the sheet drawn hot or welded to a base in an inert-gas arc.
  • Using it: heat by induction (Electric Kilns and Furnaces), always in nitrogen or argon above about 1,000 °C (Liquid Air, Nitrogen and the Noble Gases); in air it slowly burns away.

Platinum–iridium. Easier and more useful at first: platinum with 10–20 % iridium, melted together, is much harder and stiffer than platinum. It makes crucibles and dishes that keep their shape, springs, electrical contacts, surgical needles, and standards of weight and length (Measurement from Scratch).

Palladium catalyst and hydrogen purifier

Palladium on charcoal

  1. Dissolve 5 g of palladium sponge in warm aqua regia, drive off the nitric acid with hydrochloric acid, and dilute to 200 ml.
  2. Stir in 95 g of acid-washed Activated Charcoal and let it soak an hour.
  3. Reduce: make it alkaline with sodium carbonate and add formaldehyde solution (Methanol and Formaldehyde) slowly, warming gently; or later, reduce with hydrogen. The palladium is deposited as tiny particles on the carbon.
  4. Filter, wash free of chloride, and keep it damp in a closed jar. This is "5 % palladium on carbon".

A few grams of it, shaken with an oil or an organic compound under hydrogen at room temperature and 1–4 bar, adds hydrogen to its double bonds: for hardening fats, refining medicines and dyes, and many steps of Organic Synthesis and Fine Chemicals. Platinum and palladium catalysts later clean the exhaust of engines (The Motor Vehicle).

The hydrogen purifier

A thin wall of palladium lets only hydrogen pass, if it is hot. Pure palladium cracks after a few cycles of hydrogen; an alloy with 23–25 % silver does not.

  1. Draw a tube of palladium–silver alloy 2–3 mm across with a wall of 0.1–0.15 mm, closed at one end, its open end brazed into a steel fitting (Metal Pipes and Tubes).
  2. Mount it inside a steel jacket with an electric heater, keeping it at 350–450 °C.
  3. Feed impure hydrogen to the outside at 5–10 bar; draw hydrogen of better than 99.999 % purity from the inside, for semiconductor work, gas chromatographs and particle accelerators (Semiconductors and the Transistor, Chromatography, Particle Accelerators (Overview)). Bleed the impurities off continuously.
  4. Never let hydrogen touch the tube below about 300 °C. Heat it under nitrogen first and cool it under nitrogen.

A good purifier holds full vacuum on the inside when cold and passes hydrogen freely when hot. A tube that passes air has a crack.

Palladium in dentistry and jewellery

White gold is gold with about 10–20 % palladium. Dental crowns and bridges are cast by the lost-wax method (Jewellery, Beads and Medals, Dentistry) from palladium–silver (roughly half and half, with a little tin) or gold–palladium alloys. Palladium alloy contacts lasted decades in telephone relays (The Automatic Telephone Exchange).

How to tell it worked

  • Palladium salt is lemon-yellow and dissolves in ammonia with no blue tint; the metal dissolves in hot nitric acid. Rhodium solution is rose-red; iridium salt dark red-black; both metals ignore boiling aqua regia.
  • Weigh every product and residue: the total should match what went in within a few per cent.

Note Troubleshooting. Palladium salt brownish or greenish → copper or iron left in. Dissolve in ammonia and reprecipitate again. Rhodium fusion gives little colour → not hot enough, or too little bisulfate. Use more and fuse longer, at a dull red. Thermocouple reads low and keeps drifting down → contaminated wire, usually from silica or a smoky flame. Fit a gas-tight alumina sheath; cut off and re-weld. Pen tip scratches → tines uneven or edges sharp. Align under a lens and polish more.

Dangers

Danger Osmium tetroxide. Whenever osmium-bearing residues meet heat in air, chlorine, nitric acid or any strong oxidiser, they give off osmium tetroxide, a vapour that smells sharp like chlorine. It stains and destroys the eyes, causing blindness, and floods the lungs, at levels far too low to see; the usual workplace limit in air is about 0.0002 parts per million (two parts in ten thousand million). It passes through rubber. Never roast, heat or acid-boil osmiridium except in the open air or a strong draught, upwind, with goggles, and with the gases led through a trap of caustic soda and alcohol. A filter paper wetted with alcohol that turns black over a vessel means osmium is escaping. Ruthenium tetroxide, formed the same way, can also explode when warmed.

Danger Aqua regia, chlorine and fused bisulfate give choking gases and terrible burns (Nitric Acid, Chlorine and Bleach). Work outdoors, upwind, in goggles and gloves.

  • Platinum-metal salt allergy: chloro-salts of platinum and its sisters cause asthma and rashes that worsen with every exposure (Platinum and the Platinum Metals). Handle them damp and gloved.
  • Catalysts catch fire. Dry palladium on carbon and palladium sponge loaded with hydrogen glow and ignite solvent vapour and hydrogen. Keep them wet, never add them dry to a flammable liquid, and blanket with nitrogen.
  • White heat: oxy-hydrogen melting needs dark welding glasses (Welding).

What this unlocks

Furnace temperatures read to the top of the steel, glass and ceramic range (Very-High-Temperature Furnaces, The Electric Arc Furnace, Optical Glass and Achromatic Lenses); hydrogenation in Organic Synthesis and Fine Chemicals and Making Medicines; ultrapure hydrogen for Semiconductors and the Transistor and Making Microchips; crystals for Lasers and Synthetic Gems; durable fountain pens, mirrors, contacts and dental work.

How it was first done

In London in 1802, William Hyde Wollaston, working the liquors left from his platinum refining with Smithson Tennant, found palladium; he sold it anonymously as "new silver" in a shop in Soho in 1803, which caused a scandal among chemists before he owned up. In 1804 he found rhodium, named from the Greek for rose, after its salts. Tennant found osmium (from the Greek for smell) and iridium (from the rainbow, after its many-coloured salts) in the black insoluble residue in 1803–1804. Karl Klaus of Kazan found ruthenium in Ural platinum in 1844. Gold pens tipped with grains of osmiridium appeared in England in the 1830s, and made the fountain pen practical. Henri Le Chatelier introduced the platinum–rhodium thermocouple in 1886; the 13 % rhodium type R followed, and the type B couple of two rhodium alloys came from German makers in the 1950s. The international prototype kilogram, made in 1889, was platinum with 10 % iridium, and served as the world's standard of mass until 2019.

Source: content/entries/metals/platinum-group-metals.md