◆ Rebuild

Part 3 · Metals

Leaching, Solvent Extraction and Electrowinning

Get copper out of rock too poor to smelt, with no furnace at all. Trickle dilute sulfuric acid through crushed ore in vats or heaps until it runs out blue, then win the copper back by letting it plate onto scrap iron in a trough, or by electric current in a tank of lead and steel plates, after cleaning the liquor with an extractant in kerosene. How to test an ore, build a leach heap, a cementation launder and an electrowinning cell, why cyanide leaching of gold is left out of this book, and how to keep acid out of the rivers.

Difficulty
●●●●●
Time
An afternoon for a bottle test; weeks to months to leach a heap; a day to build a launder; a week to build and start an electrowinning cell
Steps from zero
26 prerequisites →

You need first

Finding and Identifying OresSulfuric AcidEDTA, Extractants and Chelating Agents

This unlocks

—
The full path from nothing — 26 steps before this one
  1. Fire
  2. Stone Tools
  3. Finding and Preparing Clay
  4. Finding and Identifying Ores
  5. Sulfur
  6. Simple Machines
  7. Pottery
  8. The Kiln
  9. Quarrying and Cutting Stone
  10. Lime
  11. Mining and Tunnelling
  12. Lye and Potash
  13. Fermentation
  14. Glass
  15. Saltpeter
  16. Distillation
  17. Acids, Bases and Testing
  18. Coal and Coke
  19. Sulfuric Acid
  20. Coal Tar Chemicals
  21. Laboratory Glassware
  22. Organic Synthesis and Fine Chemicals
  23. Identifying Substances
  24. Nitric Acid
  25. Rare Earths, Cerium and Phosphors
  26. EDTA, Extractants and Chelating Agents
  27. Leaching, Solvent Extraction and Electrowinning

Do them roughly in this order. See it on the tech tree →

Why it matters

Smelting copper needs rich ore, a lot of charcoal and a hot furnace (Copper Smelting). Most copper-bearing rock is far too poor, holding 5–20 kg of copper a tonne. Old mines leave dumps of it, and drain blue-green water that poisons the streams.

Hydrometallurgy (metal-winning with water) gets that copper out cold. Weak acid dissolves it; the blue liquor is collected; scrap iron or electric current pulls the copper out. It needs no fuel to melt rock, works with barrels and troughs, scales up to a fifth of the world's copper, and cleans mine water instead of leaving it to the rivers.

The same ideas, leach, purify, recover, give zinc, nickel, cobalt, alumina and rare earths (Separating the Rare Earths, Alum and Alumina).

How it works

Dissolving. The green and blue copper minerals of the weathered top of a deposit (malachite, azurite, chrysocolla, cuprite) dissolve in dilute Sulfuric Acid, giving copper sulfate, the blue salt also called bluestone. Each kilogram of copper dissolved uses at least 1.5 kg of acid; in practice 2–5 kg, because the rock eats some.

Sulfide ores dissolve only slowly. Chalcopyrite and other sulfides need an oxidiser as well as acid. In damp heaps open to air, the iron in the ore turns to ferric sulfate, which attacks the sulfides, and natural bacteria that live in acid water speed this up many times. It takes months to years, but it is how most of the copper in old mine water got there.

Keep it acid. Hold the liquor at about pH 1.5–2.5 (pH, Indicators and Buffers). Above about pH 3, iron comes out of solution as rusty slime that blocks the heap.

Limestone is the enemy. Rock full of limestone or dolomite eats acid and makes gypsum that clogs everything. If the ore fizzes strongly with acid, acid leaching will cost more acid than the copper is worth (ammonia leaching suits such ore, in outline below).

Getting the copper back. Three ways, from simplest:

  • Cementation: iron dissolves and copper comes out in its place as a red powder. Each 56 g of iron could, in theory, give 63.5 g of copper; in practice ferric iron and free acid also eat iron, and you use 1.5–2.5 kg of iron per kg of copper.
  • Solvent extraction: an oily extractant in kerosene picks copper out of the dirty liquor and hands it over to a clean, strong acid (EDTA, Extractants and Chelating Agents).
  • Electrowinning: current plates pure copper from that clean liquor onto a cathode, while water is split at an insoluble anode, releasing oxygen and regenerating the acid. It takes about 2 volts, and each ampere-hour gives 1.19 g of copper (Faraday's law, Electrolysis): about 2 kWh per kilogram.
Raffinate topped up with acid, pumped back Dilute acid drips on top 5–15 g/L, 5–10 L per m² per hour Crushed ore heap under 2–5 cm, 2–6 m high Gravel drain and pipes Clay and plastic liner rammed clay 30 cm; slope 2–5 % Pregnant solution pond 1–6 g of copper per litre To copper recovery pump
Fig. 1 Heap leaching. Crushed ore is stacked on a sloping pad lined with clay and plastic, over a gravel drain with pipes. Dilute acid drips onto the top, trickles down through the ore and collects in the drain. The blue copper-bearing solution flows to a lined pond, from which it goes to copper recovery; the stripped solution is topped up with acid and pumped back to the heap.

What you need

Item Amount See
Oxidised copper ore, crushed 1 kg for a test; tonnes for a heap Finding and Identifying Ores, Ball Mills, Crushers and Grinders
Sulfuric acid 2–5 kg per kg of copper Sulfuric Acid
Clay, and tar or plastic sheet Liners for pads, ponds and launders Finding and Preparing Clay, Tar, Pitch and Glue, Petrochemicals and Modern Plastics
Gravel and perforated pipe Heap drains Tiles and Clay Pipes
Scrap iron: thin sheet, old cans, turnings 1.5–2.5 kg per kg of copper Tins, Cans, Drums and Tanks
Hardwood planks Vats and launders Barrels and Cooperage
Lead sheet, stainless steel sheet Electrowinning anodes and cathodes Lead, Alloy and Stainless Steels
Direct current supply, 2–3 V per cell, tens to hundreds of amperes Electrowinning Rectifiers: Turning AC into DC, The Generator
Lime or limestone Neutralising waste liquor Lime
pH papers or indicator, a balance, a hydrometer Control pH, Indicators and Buffers, Measurement from Scratch

Where to find it

  • The oxidised cap of a copper deposit: the top few metres to tens of metres, where rain and air have rotted the sulfides. Look for green malachite, blue azurite, red cuprite, and blue-green, waxy chrysocolla, which sticks to a wet tongue. Below lies grey, brassy chalcopyrite (Finding and Identifying Ores).
  • Old dumps and tailings, especially green-stained ones.
  • Blue or green mine water from adits and dumps. Hang a bright iron nail in a cup of it overnight: a pink-red coat of copper means copper worth recovering.

Field test of an ore. Crush a spoonful, cover it with a few times its volume of dilute acid (one part strong acid to ten of water, poured acid into water), wait an hour. A blue liquid means acid-soluble copper. Then dip a nail: it turns pink. Violent fizzing means limestone: a poor prospect.

Testing before you build

  1. Bottle test. Crush 1 kg of ore to under 2 mm. Put it in a large jar with 2 litres of water containing 20 g of strong sulfuric acid per litre. Roll or shake it now and then for two days, checking the pH and adding acid to keep it near 2. Record how much acid you added.
  2. Measure the copper in the filtered liquor by cementation: hang a weighed piece of clean iron in a measured volume, warm it gently until a fresh nail no longer turns pink, then wash, dry and weigh the red copper (Identifying Substances).
  3. Judge it. Copper dissolved ÷ copper in the ore (by fire assay, Gold and Silver) is the recovery: aim for 60 % or more. Acid used ÷ copper dissolved should be under about 5. A heap of coarser rock does worse than the bottle.
  4. Column test for a heap: a pipe 15 cm across and 1–2 m tall of heap-size ore, trickled with acid for six to eight weeks, shows how fast copper comes and whether it clogs.

Method 1: The leaching vat

For a few tonnes of rich oxide ore, or as a first plant.

  1. Vats. Square wooden tanks about 1.5 m each way and 1 m deep, tarred or lined with lead or plastic, each with a false bottom of slats covered by coarse sacking, and a tap below it (Barrels and Cooperage, Lye and Potash). Or concrete tanks painted inside with hot bitumen. A cubic metre holds about 1.6 tonnes of crushed ore.
  2. Crush the ore to about 1 cm and screen out the dust, which slows the flow; mix the dust with a little strong acid and water into lumps and add those.
  3. Leach in series. Line up four to six vats. Fresh acid (30–50 g per litre) goes first onto the most nearly finished ore, then the liquor passes on, vat by vat, to the freshest ore. Strong acid meets weak ore; weak, copper-laden liquor meets fresh ore and leaves rich. Change the order every few days, emptying the oldest vat and refilling it.
  4. Wash each finished vat with water before digging it out. Oxide ore at 1 cm gives up 80–90 % of its copper in one to two weeks.

Method 2: The leach heap

For large tonnages of poorer ore. A heap is a vat with no walls, leaching for months.

  1. Site. Firm ground sloping 2–5 % towards a pond site, away from streams and wells, above flood level (Surveying and Levelling).
  2. The pad. Lay 30 cm of clay, damp and rammed in two layers (Dams and Reservoirs), then if you can plastic or tarred felt with sand above. Any leak reaches the groundwater.
  3. Drains. Lay perforated pipes of clay or plastic down the slope every 3–5 m, in a 30–50 cm blanket of washed gravel, all running to a collecting ditch at the low edge.
  4. Stack the ore, crushed to under 2–5 cm, in a flat-topped heap 2–6 m high, dumped from the top and never driven over, so it stays loose. Mixing in 5–15 kg of strong acid per tonne, with water, as you stack it (acid curing) sticks the fines into lumps and starts the leach.
  5. Irrigate. Spread dilute acid (5–15 g per litre) over the top through perforated pipes or drippers at about 5–10 litres per square metre per hour, roughly a heavy rain. Do not flood it: water must trickle through air spaces, not stand.
  6. Collect. The pregnant solution that runs from the drains carries 1–6 g of copper per litre. It goes to a lined pond and on to recovery. The spent liquor (raffinate) is topped up with acid and goes back on the heap.
  7. Ponds. Line every pond like the pad, and build a separate storm pond big enough to hold the run-off of the heaviest rain you have known, so a storm never washes acid into a stream.

Timetable. Oxide ore gives 60–80 % of its copper in two to four months. Sulfide ore gives a little each year for many years, helped by bacteria, if air reaches it between wettings.

Good versus bad heap. A good heap drains evenly, the outflow is blue and clear, and its copper content falls slowly over weeks. A bad heap shows ponds on top and wet, slumping sides (fines or clay blocking it), or the outflow turns rusty and the pH rises (acid being eaten, iron precipitating).

Method 3: The cementation launder

The simplest way to get metal from blue liquor, used since the Middle Ages.

Blue copper solution in Baffles: over and under so the liquor touches all the iron Thin scrap iron kept under the liquid Red cement copper settles washed out through gates every few days Bright nail in the last bay stays bright when the copper is out Pale green ferrous sulfate crystallise or neutralise slope about 1 cm per metre
Fig. 2 The cementation launder. Blue copper solution runs slowly down a sloping wooden trough filled with scrap iron, held between cross baffles that make it flow over and under. Red cement copper settles in the bottom of each bay. The solution leaves pale green, as ferrous sulfate, and a bright nail in the outlet stays clean when all the copper is out.
  1. The launder (an open trough for liquid). Plank, tarred or pitched inside, 40–60 cm wide, 30–40 cm deep, and 10–30 m long, in sections, sloping about 1 cm per metre. Or a series of tarred pits or tanks stepping down a slope.
  2. Baffles. Every metre, a cross board alternately rising from the floor and hanging from the top, so the liquor must pass over and under and touch all the iron. Each bay has a plug hole or a sliding gate in the bottom for washing out.
  3. The iron. Fill the bays with thin scrap: sheet, old cans (burn off paint and tin in a bonfire first), turnings. The thinner the iron, the more surface and the faster the work. Iron must stay under the liquid.
  4. Flow. Run the liquor through slowly, so that it spends an hour or two in the launder. Too fast, and copper escapes in the outflow.
  5. Check the outlet. Hang a bright nail in the last bay. If it stays bright after ten minutes, the copper is out. If it turns pink, slow the flow or add iron.
  6. Harvest every few days. Lift and shake the iron, stop the flow, open the bay gates and wash the red sludge into a settling box. Wash it with water until the washings are no longer green, dry it, and you have cement copper, 70–90 % copper, the rest iron and dirt.
  7. Refine it by melting under charcoal in a crucible (Copper Smelting, Metal Casting), then if needed by electrolysis (Electrolysis).
  8. The outflow is a solution of ferrous sulfate, green vitriol. Do not let it run away: evaporate it in lead or iron pans to crystallise green vitriol for ink, dyeing or Sulfuric Acid, or neutralise it with lime (below).

Good versus bad cement copper. Good cement is a fine brick-red to salmon powder that shines copper when rubbed with a knife. Black, sticky cement full of rust means too little acid, or iron left in too long.

Method 4: Solvent extraction (in outline)

Cementation eats iron and gives impure copper. Solvent extraction cleans the liquor instead: an oxime extractant in kerosene, stirred with the pregnant solution in a mixer-settler (a stirred box overflowing into a long settling tank), takes the copper and leaves the iron; strong acid from the cells strips it back as clean liquor of 45–50 g of copper per litre. Chemistry and drawing are in EDTA, Extractants and Chelating Agents, cascades in Separating the Rare Earths.

Method 5: The electrowinning cell

DC 2 V + − + bus bar touches every anode Lead anode does not dissolve; gives off oxygen Stainless steel cathode copper grows on both faces, stripped off every 5–7 days − bus bar touches every cathode Insulator under each cathode hanger on this side Floating balls hold down acid mist Electrolyte 35–50 g/L copper, 150–180 g/L acid, 45 °C
Fig. 3 An electrowinning cell, cut away. Lead alloy anodes and stainless steel cathodes hang alternately from copper bus bars on the tank walls, all anodes on the positive bar, all cathodes on the negative. Pure copper plates onto both faces of each cathode, oxygen bubbles rise from the anodes, and a layer of floating plastic balls holds down the acid mist.
  1. The tank. Acid-proof: wood or concrete lined with lead sheet, polythene or fibreglass, or a large glazed stoneware vessel. A small cell: 100 litres, about 80 cm long, 40 cm wide, 50 cm deep.
  2. Anodes. Rolled lead sheet 6–8 mm thick, alloyed with a little tin and calcium, or with 6 % antimony, to stay stiff and resist corrosion (Lead, Antimony and Bismuth). Unlike refining, the anodes do not dissolve; they make oxygen.
  3. Cathodes. Polished stainless steel sheet, with plastic strips along the side edges so the copper does not grow round them, and the plated copper is peeled off each crop. Or thin pure copper starter sheets that become part of the product, made as in Electrolysis.
  4. Spacing. Hang anode, cathode, anode … with 4–5 cm between each anode and the next cathode, cathodes a little larger than anodes. Every anode hangs from the positive bus bar, every cathode from the negative, with clean, bright contacts.
  5. The electrolyte. Clean liquor of 35–50 g of copper and 150–180 g of sulfuric acid per litre, kept at 40–50 °C. Without solvent extraction, use liquor low in iron (under about 1–2 g per litre): ferric iron is reduced at the cathode and re-oxidised at the anode, wasting current. A trace of cobalt sulfate (about 0.1 g per litre) slows anode corrosion, and a pinch of glue or plant gum (about 0.01 g per litre) keeps the copper smooth (Glues and Adhesives).
  6. Current. About 2.5–3 A per dm² of cathode face (counting both sides). The cell settles at 1.9–2.2 V. With three cathodes of 30 × 30 cm in the small cell (0.54 m² of face), that is about 135 A, some 300 watts, making about 3.5 kg of copper a day.
  7. Circulate the liquor slowly and keep its copper above about 30 g per litre, or the cathodes grow dark, spongy copper and give off hydrogen.
  8. Mist. Oxygen bubbles throw up a fine acid mist: float plastic or waxed-cork balls on the surface and ventilate.
  9. Harvest after 5–7 days, when the copper is about 4–6 mm thick each side: lift the cathodes, wash them, and flex or knock them to strip the copper sheets. The spent liquor, richer in acid, goes back to stripping or to the heap.

Electrowon copper of a good cell is 99.9 % or purer, good enough to cast and draw into wire directly (Copper Wire).

Good versus bad cathode. Good copper is salmon-pink, dense and smooth, with no lumps at the edges and no dark patches. Nodules and branching "trees" that reach for the anode mean too high a current, too little additive or solid particles in the liquor. Dark, powdery copper means too little copper in the liquor or too much current. Grey streaks are lead flaking from the anodes.

Other metals and leaches (in outline)

  • Zinc: roasted concentrate leached in sulfuric acid, purified strictly (traces of cobalt or antimony ruin it), and electrowon onto aluminium cathodes at about 3.3–3.5 V (Zinc and Brass).
  • Ammonia with air dissolves copper as a deep-blue complex and leaves limestone untouched: the answer for limy ores and scrap (Ammonia).
  • Nickel and cobalt from laterite clays need acid in autoclaves at 250 °C (Nickel and Cobalt); alumina comes from bauxite in hot caustic soda (the Bayer process, Aluminium).

Cyanide leaching of gold: history and hazard only

Danger This book gives no working method for cyanide leaching, deliberately. Cyanide is among the fastest-acting poisons there is: a few hundred milligrams of its salts kill an adult, and if a cyanide solution becomes even slightly acid it gives off hydrogen cyanide gas, which kills in minutes in a closed space. Safe use needs constant chemical monitoring, alkaline control, destruction of every drop of waste, antidotes and trained medical staff on site, and a works designed so that no spill can reach water. A rebuilding community does not have these, and a single mistake poisons people and a river for a generation.

What it was. In 1887 in Glasgow, John Stewart MacArthur with the brothers Robert and William Forrest patented dissolving gold from crushed ore with a weak solution of cyanide and air. Within a few years it was rescuing the gold fields of New Zealand and the Witwatersrand in South Africa, where much of the gold was too fine to catch by washing, and it became the standard gold process of the 20th century.

What it did. Cyanide spills have killed rivers. In January 2000, a tailings dam at Baia Mare in Romania overflowed, sending about 100,000 m³ of cyanide-laden water into the Someș, Tisza and Danube rivers and killing fish for hundreds of kilometres downstream. Small gold diggings that use cyanide and mercury together still poison workers, their children and their rivers today (Mercury).

Use instead: panning, sluices, jigs and shaking tables to catch free gold (Gold and Silver, Ore Dressing: Jigs, Tables and Flotation), and smelting the concentrate with lead followed by cupellation. They recover less of the finest gold, and they do not kill.

Caring for the land and water

  • Line every pad and pond, keep a storm pond, and check them after heavy rain. Dig a test well downhill of the heap and test it monthly: blue colour, a pink nail or a pH below 5 means a leak.
  • Neutralise every waste liquor before release: stir in lime or crushed limestone (Lime) until the pH reaches 7–8. Iron and copper fall out as a mud of hydroxides and gypsum. Let it settle in a lined pond, run off the clear water, and bury the mud in a lined, capped pit.
  • Closing a heap. Rinse it with water until the outflow is nearly neutral, then lime-wash it, cover it with a layer of clay and topsoil, and plant grass (Understanding Soil). An unclosed heap of sulfide rock makes acid for centuries.

How to tell it worked

  • Pregnant liquor is clear and blue; a nail in the launder outflow stays bright.
  • Weigh the copper won weekly against the copper dissolved (litres × grams per litre). For a cell, copper ÷ (amperes × hours × 1.19 g) is the current efficiency: aim for 85–95 %.
  • The downhill test well stays clear and neutral.

Note Troubleshooting. Heap stops draining, ponds on top → too many fines or clay. Agglomerate with acid before stacking; rip the top with a fork; irrigate less. Outflow orange, pH above 3 → acid eaten by limestone, iron precipitating. More acid, or abandon that ore for ammonia leaching. Little copper in the liquor → sulfide ore, or ore too coarse. Crush finer; leach longer with air; test with a column. Launder eats iron but makes little copper → liquor too acid or rich in ferric iron. Pass it over waste iron first, or reduce acid. Cell voltage rising → bad contacts on the bus bars, or cold liquor. Clean contacts; warm it. Cathodes short-circuit → nodules touching anodes. Lower current, add gum, filter the liquor, straighten the plates.

Dangers

Danger Sulfuric acid burns skin and blinds. Always pour acid into water, never water into acid; wear goggles, rubber gloves and boots, and keep plenty of water at hand (Sulfuric Acid). Leach liquor at 10–20 g per litre is weak but still hurts eyes and cuts; electrolyte at 180 g per litre is strong acid.

Danger Arsine. If the ore contains arsenic (Arsenic), acid liquor meeting iron or zinc can give off arsine, a colourless gas smelling faintly of garlic that destroys the blood. Test ores for arsenic before leaching; run launders in the open air, never in sheds or pits; anyone with headache, dark urine or yellowing skin after working the launder needs a doctor at once.

  • Acid mist from electrowinning cells corrodes lungs and teeth. Cover the cells, float balls on them, ventilate.
  • High current. The voltage of a cell is low, but hundreds of amperes through a ring, watch or spanner across a bus bar burn to the bone. Remove metal jewellery.
  • Lead anode scale is poisonous (Lead); kerosene in the settlers burns fiercely; ponds are steep and slippery: fence them.

What this unlocks

Copper from ores no furnace could use, at village scale, for Copper Wire, motors, generators and Electroplating. Bluestone for batteries and as a fungicide on vines and potatoes (Pests and Plant Diseases). The same leach–purify–electrowin idea gives zinc, nickel and cobalt, and the clean water skills of Water Treatment for a Town and Rubbish, Recycling and Reuse. It is also a tool for cleaning up: copper recovered from mine drainage is copper kept out of the fish.

How it was first done

In Song dynasty China, from about the 11th century, copper was won on a large scale by soaking scrap iron in "bitter" mine waters in channels and pits, and for a time this probably supplied a significant share of the empire's copper. In Europe, the "cement waters" of the Hungarian mines at Herrengrund (now Špania Dolina in Slovakia) were worked from the 16th century, and at Parys Mountain on Anglesey, in the 18th century, mine water ran through iron-filled pits. Heap leaching of copper ore was practised at Rio Tinto in Spain from the 18th century. In 1915 the Chuquicamata mine in Chile began leaching oxide ore with sulfuric acid and electrowinning the copper, and electrolytic zinc plants opened in Montana and British Columbia the same year. The bacteria that turn iron and sulfur into acid in mine water were identified in 1947. Solvent extraction of copper with oxime extractants was first used commercially at the Bluebird mine in Arizona in 1968, and leaching with solvent extraction and electrowinning now produces about a fifth of the world's copper.

Source: content/entries/metals/hydrometallurgy.md