How to get salt from seawater, salty springs and rock salt — by sun, by fire, or both — and how to purify it. Salt keeps people alive, preserves food through winter, and is a raw material for much of chemistry.

Difficulty
●●●●●
Time
1–3 weeks by sun; a day of boiling for a few kilograms
Steps from zero
3 prerequisites →

You need first

FirePottery

This unlocks

Bromine and BromidesChlorine and BleachHydrochloric AcidSoda Ash and Baking SodaElectrolysisDairy and CheesePreserving FoodSausages, Ham and BaconVinegar and PicklingOral RehydrationMagnesium

Objects made here

salt panboiling pan
The full path from nothing — 3 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Pottery
  4. Salt

Do them roughly in this order. See it on the tech tree →

Why it matters

Your body cannot work without salt. Sodium carries nerve signals, holds water in your blood and lets your muscles move. You lose it in sweat and urine every day. People who eat a lot of fresh meat and blood get enough from their food; people who live on grain and vegetables, or who sweat heavily in heat or hard work, need added salt or they become weak, cramped, dizzy and confused.

Salt also lets you keep food. Meat, fish, cheese and vegetables packed in salt or soaked in strong brine stop rotting, because the salt pulls water out of them and out of the bacteria that would spoil them. Before refrigeration, salt was the difference between a winter of plenty and a winter of hunger. See Preserving Food and Dairy and Cheese.

And salt is a chemical: it cures hides for Hides and Leather, and later becomes Hydrochloric Acid, Soda Ash and Baking Soda (for Glass and Soap), and, by Electrolysis, Chlorine and Bleach.

How it works

Seawater is about 3.5% dissolved salts — about 35 grams in every litre. Most of that (about 27 g) is common salt, sodium chloride. The rest is mainly magnesium and calcium salts.

Salt dissolves easily in water, up to about 360 grams per litre. Almost exactly the same amount dissolves in hot water as in cold, so you cannot get salt out by cooling brine. You must remove the water — by sun and wind, or by boiling. As the water goes, different substances come out of solution at different stages:

Brine left (of the starting seawater) What comes out
About 1/2 A tiny amount of chalky calcium carbonate
About 1/5 to 1/4 Gypsum (calcium sulfate) — soft, white, not salty. Settles as a crust or sludge
About 1/10 Common salt starts to crystallise. Keep going
About 1/30 and less Bitter salts (magnesium salts) — bitter-tasting, damp, laxative. The leftover liquid is called bittern. Pour it off; do not dry it with your salt

So the art of salt-making is: concentrate the brine, let the gypsum drop out, crystallise the salt, and stop before the bittern dries onto it.

Brine strength without instruments. A fresh egg sinks in seawater, but floats in brine about three times as strong. When the egg floats, your brine is worth boiling. In nearly saturated brine (ready to crystallise), the egg floats high, with a patch the size of a coin above the surface.

What you need

Item Amount Notes
Seawater, spring brine or rock salt See methods One litre of seawater gives about 25–30 g of salt
Flat ground near the source For solar pans Clay soil, or ground you can line with clay
Clay For lining pans and making boiling pots See Finding and Preparing Clay
Wide, shallow fired pots or clay pans Several Shallow pans boil faster than deep pots. See Pottery
Fuel Plenty Boiling takes a lot of wood (below)
Baskets or cloth Several For draining crystals and filtering
Clean sand For the sand method
A fresh egg 1 For testing brine

Where to find it

  • The sea. Any coast. Rocky shores often have pools where the sun has already concentrated seawater, sometimes leaving a crust of salt crystals on the rocks — collect it.
  • Salt springs. Inland, look for springs or seeps where the water tastes salty, where white crusts form on the ground, where animals gather to lick the earth ("salt licks"), and where salt-loving plants grow far from the sea — glasswort (fleshy, jointed, leafless green stems that turn red in autumn), sea-blite and saltbush. Many ancient towns grew up beside salt springs.
  • Rock salt (halite). In dry regions, salt lies in thick beds underground and sometimes comes to the surface in hills, cliffs and the floors of dry lakes. It looks like glassy, colourless, white, grey or pinkish rock, breaks into cubes, dissolves in water, and tastes clearly salty. Salt flats in deserts are crusts of salt left by dried-up lakes.
  • Dry lake crusts that taste soapy or bitter, not salty, are other salts: a soapy, slippery taste means soda (useful for Glass and Soap — see Soda Ash and Baking Soda); a bitter taste means sulfates or magnesium salts. Do not eat them.

Method 1: Solar salt pans

In a hot, dry, windy season the sun does all the work. This is how most of the world's sea salt has always been made.

Sun and windtake off 5–10 mm of water a day Sealet in at high tide Concentrating panslargest, 10–20 cm deep Middle pansgypsum settles out Crystallising pans3–5 cm; salt forms Rake updrain, dry floors of trampled clay so no brine soaks away
Fig. 1 Solar salt pans. Seawater moves from pan to pan, getting stronger as it evaporates. Gypsum drops out in the middle pans; salt crystallises in the last, shallowest pans and is raked up while still wet with brine.
  1. Choose the site. Flat ground just above high tide, with clay soil, little rain expected for several weeks, sun and steady wind.
  2. Build the pans. Make a series of shallow pans, each about the size of a room or smaller, with low earth banks 15–20 cm high. Puddle the floors: wet the clay soil, trample it smooth and hard, and let it dry, so water cannot soak away. If the soil is sandy, line the floor with 5 cm of trampled clay. Make three or more rows:
    • Concentrating pans — biggest, 10–20 cm deep.
    • Middle pans — where the brine gets strong enough to drop gypsum.
    • Crystallising pans — smallest, 3–5 cm deep, with the smoothest, cleanest floors.
  3. Fill and move. Let seawater into the first pans (at high tide, through a gap you can block, or by carrying it). Every few days, as it evaporates and gets stronger, move the brine on to the next pan by opening a gap or by bucket, and refill behind it. Test with an egg.
  4. Crystallise. When the brine is near saturation (the egg floats high), let it into the crystallising pans. Within days a crust of salt forms on the surface and sinks; crystals grow on the floor.
  5. Harvest while wet. When there is a good layer of crystals but still some brine over them, rake the salt into heaps on the pan edge to drain. Do not let a pan dry right out — that dries the bitter salts onto your salt. Drain the bitter leftover liquid away from your pans and fields.
  6. Dry and store the drained salt in the sun on a mat, then in closed pots or baskets under cover.

How much? Each square metre of crystallising pan holds about 50 litres at 5 cm deep, and gives about 1.3 kg of salt when dried down. In hot, dry weather, seawater loses about 5–10 mm of depth a day, so 5 cm takes one to two weeks.

Method 2: Boiling

Where the weather is not hot and dry enough, or when you need salt now, you boil the brine. Boiling raw seawater costs a great deal of fuel — roughly half a kilogram to a kilogram of dry wood for every litre of water boiled away, which means 20–40 kg of wood for each kilogram of salt. So always strengthen the brine first.

1 · MAKE STRONG BRINE 2 · BOIL IT DOWN Pour seawaterthrough, slowly Filterbasket linedwith grass Salty sandcrusted by sunafter 1–3 days Strong brinea fresh eggfloats in it Shallow pansskim the scum Draining basketcrystals scooped in,brine drips back long trench fire under the pans
Fig. 2 Making brine with sand, and boiling it down. Seawater poured over sand that the sun has already crusted with salt washes out a brine five or more times stronger than the sea. That brine is boiled in shallow clay pans until salt crystals form.

Step 1: Make strong brine (the sand method)

This is an ancient method, still used in Japan and once common on the coasts of Europe.

  1. On a flat, clay-floored area near the shore (or on the upper beach), spread clean sand 1–2 cm thick.
  2. Sprinkle or splash seawater over it several times a day. The sun and wind dry it, leaving salt stuck to every grain. After one to three days the sand looks dull and crusty and tastes very salty.
  3. Scrape up the salty sand and pile it into a filter: a basket lined with grass or cloth, or a clay-lined pit with a hole at the bottom, set over a pot.
  4. Pour seawater (not fresh water) through it slowly. It dissolves the salt from the sand and runs out as strong brine — five or more times as strong as seawater. Test with an egg. Spread the washed sand out again and repeat.

You can also use the first solar pans (Method 1) to strengthen brine even in a poor season, then finish by boiling. Salt-spring brine is often already strong.

Step 2: Boil it down

  1. Settle the brine. Let it stand in a pot overnight, then pour it off the mud and sand. Filter through cloth if cloudy.
  2. Use wide, shallow pans. Shallow clay dishes 5–10 cm deep, or the widest pots you have, set over a long trench fire or on stones over the fire. Shallow pans evaporate far faster than deep pots.
  3. Boil hard at first. Skim off the grey scum as it rises. Keep topping up with more brine.
  4. Watch for gypsum. A thin white crust forms on the bottom and sides of the pan (scale). That is mostly gypsum. If you can, let the brine cool, pour it off into a clean pan, and continue.
  5. Simmer as crystals form. When a skin of tiny crystals appears on the surface, lower the heat. Gentle heat grows larger, cleaner crystals. Scoop out crystals with a wooden or clay spoon into a basket or cloth bag hung over the pan, so the brine drips back.
  6. Stop before dryness. When the remaining liquid is a small fraction of what you started with and the crystals start to taste bitter, stop. Throw the bitter liquid away.
  7. Dry the drained salt in the sun or beside the fire.

Tip Briquetage. Ancient salt makers often boiled brine in small, cheap, coarse clay pots, then broke the pots to get out the cakes of salt. The salt was traded in these hard cakes, which kept dry and were easy to carry and count.

Method 3: Rock salt

  1. Break out rock salt with a stone or wooden mallet.
  2. Clean pieces can be crushed and used directly.
  3. Dirty or mixed rock salt should be dissolved in water in a pot, the mud allowed to settle overnight, and the clear brine poured off and boiled down as in Method 2. This is how salt has been "mined" from underground beds for centuries: by pumping water down and bringing brine up.

Purifying salt (recrystallisation)

Crude salt is grey or brown, gritty and slightly bitter. To clean it:

  1. Dissolve it in clean water, about 1 part salt to 3 parts water by weight, stirring until no more dissolves.
  2. Settle overnight. Pour the clear brine off the sludge.
  3. Filter it through tightly woven cloth, or through a bed of clean sand and crushed Charcoal in a pot with a hole in the bottom. This removes fine dirt and some colour and smell.
  4. Boil it down gently, as in Method 2, scooping out crystals as they form.
  5. Rinse the crystals by pouring a little clean, saturated brine over them in the draining basket. It washes off the bitter liquid without dissolving the salt.
  6. Stop while a third of the liquid remains, and throw that away.
  7. Dry thoroughly and store in a closed pot.

Repeat for very pure salt (for medicine, food for infants and chemistry).

How to tell it worked

  • Taste. Clean, sharp, purely salty. A bitter after-taste means bittern (magnesium salts): rinse with saturated brine or recrystallise.
  • Dryness. Good salt stays dry and runs freely in dry weather. Salt that turns damp and sticky in humid air contains magnesium salts.
  • Look. White, with clear cube-shaped or hollow pyramid-shaped crystals. Grey or brown colour is mud — refilter.
  • Water test. A spoonful dissolves completely in a cup of clean water, leaving the water clear. Grit or cloudiness means impurities.

Note Troubleshooting. Salt is bitter or damp → bittern dried onto it; harvest earlier and rinse. Very fine powdery salt → boiled too hard at the end; simmer gently for bigger crystals. Pans leak, brine disappears → floors not puddled; trample more clay into them. Rain ruins the pans → make salt only in the dry season; keep finished salt covered.

Using salt

  • Preserving. For dry salting fish and meat, use roughly 1 part salt to 3–4 parts flesh by weight, rubbed in and layered. For brining, use brine strong enough to float an egg. Details in Preserving Food.
  • Health. A healthy adult needs at least 1–3 g of salt a day in a cool climate, and much more when sweating heavily — up to 10 g or more in hard labour in the heat. For someone with diarrhoea, salt and sugar in clean water save lives: one litre of boiled water, half a level teaspoon (about 3 g) of salt and six level teaspoons of sugar. See Oral Rehydration.
  • Iodine. Sea salt contains very little iodine. People far from the sea who eat no seafood or seaweed can develop goitre (swollen neck) and their children can be harmed. See Nutrition and Deficiency Diseases and Iodine.
  • Hides. Rubbing fresh hides with salt stops them rotting until they can be tanned. See Hides and Leather.
  • Cold. Salt mixed with crushed ice makes a mixture as cold as −20 °C — useful for freezing and for some chemistry.
  • Chemistry. Salt is the starting point for Hydrochloric Acid, Soda Ash and Baking Soda, and, with electricity, Chlorine and Bleach (Electrolysis). Thrown into a hot kiln at about 1,200 °C, it glazes stoneware (see Glazes).

Dangers

Danger Never drink seawater. It is saltier than your blood, so your kidneys need more water to get rid of the salt than the seawater gave you. Drinking it speeds up dehydration and death. The same goes for urine. Make fresh water instead (see Finding and Purifying Water and Distillation).

  • Boiling brine is hotter than boiling water and sticks to skin. Pans of boiling brine can also spit violently when a dry crust breaks, and salt crystals heated dry crackle and jump. Keep faces back, and children away.
  • Bittern is bitter and acts as a strong laxative. Pour it away from fields and drinking water.
  • Salt kills soil. Brine spilled on farmland or drained into fields poisons them for years. Keep saltworks away from crops and wells, and drain waste brine to the sea.
  • Too much salt over many years raises blood pressure and harms the heart and kidneys. Babies must not be given salty food — their kidneys cannot cope.
  • Plant-ash "salt". Some peoples far from the sea make a salty substance by burning certain plants and soaking the ash. This is mostly potassium salts and caustic alkali, not sodium chloride. It does not meet the body's need for sodium, and the alkali can burn the mouth and gut. It is not a substitute for real salt.

What this unlocks

Salt preserves meat and fish (Preserving Food), makes cheese (Dairy and Cheese), cures hides (Hides and Leather), and treats dehydration (Oral Rehydration). In chemistry, it leads to Hydrochloric Acid, Soda Ash and Baking Soda, Chlorine and Bleach and, through Electrolysis, much of the modern chemical industry.

How it was first done

People were boiling salt from spring brine at least 8,000 years ago: at Poiana Slatinei in Romania, salt makers worked a brine spring around 6000 BC, and in China, salt was gathered from Lake Yuncheng from about the same time. From the Bronze Age onward, miners dug rock salt from deep underground at Hallstatt in Austria, and coastal people all over the world made salt in pans and by boiling in clay pots. Salt was taxed, fought over and traded along special roads; Rome's Via Salaria was named after it. In 1930, Mahatma Gandhi led thousands of Indians to the sea to make their own salt, in defiance of a British tax — a simple act of salt-making that became a turning point in India's struggle for independence.