Part 5 · Cloth and Clothing
Laundry and Bleaching Cloth
How to wash a household's clothes and bedding without machines — soaking, soap and lye, beating and scrubbing, boiling and rinsing — and how to bleach grey linen white with ash lye, sunlight on grass and sour baths. Plus taking out stains, starching, ironing and keeping cloth clean between washes.
- Difficulty
- ●●●●●
- Time
- A long day for a family's weekly wash; two to six months to bleach new linen white on grass, a few weeks with an acid sour
- Steps from zero
- 5 prerequisites →
This unlocks
—The full path from nothing — 5 steps before this one
- Fire
- Finding and Preparing Clay
- Pottery
- Lye and Potash
- Soap
- Laundry and Bleaching Cloth
Do them roughly in this order. See it on the tech tree →
Why it matters
Clothes and bedding that are never properly washed carry lice, which spread typhus (Personal Hygiene, Infectious Diseases), and the mites and germs of scabies and skin infections. Clean dressings and sheets are part of Wound Care and Antiseptics and Safe Childbirth. Washing also makes cloth last: grease and grit cut fibres from inside, sweat rots them.
Washing by hand was, for most of history, the heaviest regular work in a household — a whole day a week, usually done by women, hauling and heating hundreds of litres of water. Doing it well and efficiently frees days of labour.
Bleaching turns new linen from a dull grey-brown into white. White linen is not vanity: it shows dirt so it gets washed; it can be dyed any clear colour (Dyes and Mordants); and white rags make white Paper. Bleaching was once a great industry, and the hunt for faster bleaches drove the first chemical works — Sulfuric Acid, Soda Ash and Baking Soda and Chlorine and Bleach.
Personal Hygiene gives a short everyday laundry routine. This chapter is the full craft.
How it works
Dirt in cloth is mostly three things: grease (body oil, cooking fat) which glues on everything else; protein (blood, sweat, egg, milk); and particles (soil, soot).
- Alkali — soap, or the lye from wood ash (Lye and Potash) — turns grease into a kind of soap and lifts it into the water (Soap). Warmth makes it work faster.
- Movement — rubbing, pounding, squeezing — pushes the dirty water out of the cloth and clean water in.
- Hot water sets protein stains. Heat cooks blood and egg into the fibres like boiling an egg. Always soak in cold water first; then wash hot.
- Rinsing matters as much as washing. Soap and lye left in cloth turn it grey and stiff, irritate skin and rot fibres.
Bleaching works on the natural brownish colouring of flax and cotton fibres:
- Hot lye dissolves much of the colouring and the waxes and gums still in the fibre.
- Sunlight on wet cloth in open air slowly breaks down (oxidises) the rest. Light acting on water and air makes small amounts of active oxygen chemicals, such as hydrogen peroxide, right on the fibres. The cloth must be kept wet: dry cloth in sun bleaches far more slowly.
- A sour bath — sour milk, sour bran water, or very dilute acid — neutralises the last of the lye, dissolves lime and iron stains, and brightens the white.
No single step bleaches; it is the repetition of lye, sun and sour, many times over, that whitens linen.
What you need
| Item | Notes |
|---|---|
| Water | About 15 litres per kilogram of dry laundry, for washing and two rinses. Soft water — rain or river water — is best |
| Tubs | Two or three wooden tubs of 40–80 litres (Barrels and Cooperage) |
| A copper | A big pot or cauldron of 30–60 litres for boiling, set on bricks over a fire, or built into a brick hearth (Metal Casting, Pottery) |
| Buck tub | A tall tub with a hole and bung in the side at the very bottom, on a stand |
| Soap | Soft soap, about 50–100 g per tub of washing (Soap); or soapwort for wool and silk |
| Wood ash | Clean, sifted ash of hardwood, for lye (Lye and Potash) |
| Washing tools | Washboard, dolly or posser, beetle — see below |
| Wringing | Two people, or a mangle |
| Drying | Lines and poles, a hedge, or clean grass |
| Irons | Two or three solid iron flat irons, 1.5–3 kg each (The Blast Furnace and Cast Iron, Blacksmithing) |
| Starch | Potato or wheat starch |
| Blue | A small lump of indigo tied in cloth (Dyes and Mordants) |
Where to find it
- Wood ash: burn clean, dry hardwood (oak, beech, ash, maple, fruit woods) completely to pale grey ash. Pine and other resinous woods give weaker, sooty ash. Keep it dry under cover.
- Soapwort (Saponaria officinalis): a pink-flowered plant of hedges and riverbanks whose leaves and roots, crushed and boiled, make a mild soapy lather. Gentle on wool and silk (Wool).
- Stale urine: kept a week or two in a covered pot it turns to ammonia, a strong grease-cutter. Romans washed and fulled cloth with it, and it was used for heavily soiled work clothes. Rinse very thoroughly.
- Fuller's earth and chalk: soft clays and powders that soak up grease. See Spinning and Weaving Cloth for fuller's earth.
- Sour liquids: buttermilk and whey from Dairy and Cheese; bran or meal soaked in warm water for a few days until it smells sour.
- Sorrel: sour-leaved plants of meadows and woods. The juice dissolves rust and ink stains.
- Starch: potatoes or wheat (The Great Staple Crops).
- Soft or hard water? Shake a little soap in a jar of the water. Soft water gives a good lather at once; hard water makes a greasy, curdy scum and needs much more soap. Collect rainwater from roofs (Wells and Cisterns), or soften hard water by stirring in a handful of wood ash or Soda Ash and Baking Soda per tub and letting it settle.
Washing tools
- Washboard: a hardwood board about 60 × 30 cm, with ridges carved across it 1–1.5 cm apart and 4–5 mm deep, rounded so they do not tear cloth. Stand it in the tub and rub soapy cloth up and down on it.
- Dolly: a wooden pole about 1 m long with a crosswise handle at the top and a small three- or four-legged "stool" 25 cm across at the bottom. Stand it in the tub and twist it back and forth to churn the load.
- Posser: a pole with a hollow wooden bell or cone at the bottom. Plunge it up and down: it pumps water through the clothes.
- Beetle (battledore): a flat hardwood paddle 40–50 cm long. Pound wet, soapy cloth on a smooth flat stone at the stream's edge. This is the oldest laundry tool of all and is still used in much of the world.
- Mangle: two smooth hardwood rollers 8–10 cm thick and 50–60 cm long in a frame, pressed together by wedges or a spring and turned by a crank. Folded wet cloth fed between them comes out nearly dry and half pressed. A box mangle — a heavy stone-loaded box rolled back and forth over cloth wound on rollers — presses dry sheets and tablecloths smooth without heat.
Method 1: The weekly wash
- Sort into: white linen and cotton; coloured cloth; wool and silk; very dirty work clothes and nappies.
- Mend tears first — washing makes them worse.
- Soak overnight in cold water. Rub soap into collars, cuffs and stains. Blood and milk stains go into cold salt water (a handful of Salt per bucket).
- Wash whites in hot water, as hot as hands can bear (about 50 °C), with soft soap. Rub each piece on the washboard, or churn with the dolly or posser for 10–15 minutes per tub, or pound with the beetle. Work from the cleanest to the dirtiest pieces through the same water.
- Boil whites, bedding, towels, nappies (Nappies, Feeding Bottles and Baby Gear), menstrual cloths (Menstrual Pads, Toilet Paper and Continence Care) and sickroom linen in the copper with soap for 10–20 minutes, stirring with a smooth stick. Boiling kills lice, their eggs, and most germs (Sterilising Instruments and Dressings).
- Rinse in clean water, then again. Squeeze each piece in the second rinse: if suds come out, rinse a third time.
- Blue the last rinse of whites: swish the indigo bag through it until the water is faintly sky-blue. The blue tint cancels the yellow of old linen, so it looks whiter.
- Wring — two people twisting opposite ways, or through the mangle.
- Dry in sun and wind. Whites can be spread on clean grass for extra bleaching. Bring things in as soon as dry, before evening dew.
- Coloured cloth is washed in warm (not hot) water, quickly, and dried in shade so the dye does not fade.
- Wool and silk: lukewarm water (about 30 °C, no hotter than your wrist) with soapwort or a little gentle soap, squeeze, don't rub or wring, rinse in water of the same temperature, roll in a dry cloth to take out water, and dry flat in shade. Hot water, rubbing and sudden changes of temperature felt and shrink wool (Felt).
Method 2: Bucking — washing with lye
Before soap was cheap, linen was washed in lye. It is still the best way to clean very dirty or greasy heavy linen, sheets and work clothes, and it is the heart of bleaching. Use it only on linen, hemp and cotton — lye dissolves wool and silk.
- Soak the linen overnight in cold water and wring it.
- Pack the buck tub. Put a layer of clean straw or sticks over the hole at the bottom so the cloth does not block it. Lay the linen in loosely, the dirtiest pieces at the bottom, until the tub is nearly full.
- Spread the ash cloth. Lay a coarse cloth over the top and spread on it a layer of sifted hardwood ash 3–5 cm thick (roughly a large bucketful for a tub of 60–80 litres).
- Start warm. Pour warm water (about 40 °C) over the ash. It soaks through, becomes weak lye, and runs down through the linen. Pull the bung, catch what drains out, and pour it back over the top. Do this for an hour — warm water first, so protein stains do not set.
- Get hotter. Heat the lye that drains out in the copper, a little hotter each time, and keep pouring it back over the ash and linen for 6–12 hours, ending near boiling. The liquid that runs out turns brown with dirt.
- Strength. The lye should feel just slippery between your fingers, and an egg should sink in it. Strong soap-making lye (Lye and Potash) will rot linen.
- Rinse very thoroughly — three times, or in running water at a stream — beating the cloth with the beetle. Then wash with a little soap as usual.
Method 3: Bleaching linen
New linen fresh from the The Loom is grey to brown and stiff with the size (paste) put on the warp. Bleaching it white is slow, but it needs nothing but ash, sun, grass, water and milk.
- Steep. Soak new cloth for 2–3 days in warm water or used lye to loosen the size and gums, then wash and rinse.
- Buck in lye for a day, as in Method 2.
- Croft (grass bleach). On a sunny day, spread the wet cloth flat on short, clean grass — a bleach green — and peg it down at the edges. Keep it wet: sprinkle it with water from a can or a long-handled scoop every 1–2 hours while the sun is on it. Leave it out for 3–7 days, turning it over once.
- Repeat bucking and crofting. Each round whitens a little more. Old bleachers gave fine linen 5–10 rounds, over a whole summer.
- Sour. Soak the cloth in buttermilk, sour whey, or sour bran water, enough to cover it, for 3–7 days, until it no longer smells of lye. (A modern sour is very dilute sulfuric acid, about 1 part acid to 100 parts water, for a few hours — always pour acid into water, never water into acid (Sulfuric Acid). It cut bleaching from months to weeks.)
- Wash with soap, rinse thoroughly, blue, and dry.
- Cotton is whiter to begin with and needs only two or three rounds.
For household linen that has gone yellow or grey: wash it, then lay it wet on grass in the sun and keep it damp for a day or two. Most stains and yellowing fade.
Tip Chlorine is fast but fierce. Liquid bleach made by electrolysis (Chlorine and Bleach) whitens linen in hours. Use it weak — about 1 part household-strength bleach to 20–50 parts water, for under an hour — rinse very well, and follow with a sour. Strong or long chlorine baths weaken linen and cotton badly, and chlorine destroys wool and silk.
Taking out stains
Treat stains before washing, and before any hot water.
| Stain | Treatment |
|---|---|
| Blood, milk, egg, sweat | Soak in cold salt water for hours; rub with soap; then wash. Never hot first |
| Grease, oil, tar | Cover with a paste of fuller's earth or chalk and water, leave overnight, brush off; or rub with soft soap and wash hot. Fat softens tar |
| Fruit, wine, tea | Stretch the cloth over a bowl and pour boiling water through it from a height, at once; or wet it and lay it in the sun |
| Rust ("iron mould"), iron-gall ink | Rub with crushed sorrel leaves or lemon juice and salt, lay in the sun, keep damp, repeat; rinse well |
| Mildew (grey-black spots) | Soak in sour milk, then lay on grass in the sun; badly mildewed cloth is already weakened |
| Scorch | Light scorches fade if the cloth is wetted and laid in the sun. Deep scorches are burned fibre and will not come out |
| Grass, mud | Let mud dry and brush it off; soap and wash |
Starching and ironing
Starch stiffens collars, caps, aprons and table linen and makes them shed dirt.
- Make potato starch. Grate washed raw potatoes into a bucket of cold water. Stir, then strain the pulp out through a cloth. Leave the milky water to stand for an hour: the starch settles as a white layer. Pour off the water, stir the starch with fresh water, settle again, and repeat twice until the water is clear. Spread the white starch to dry. About 1 kg of potatoes gives 100–150 g.
- Wheat starch: soak crushed wheat or flour in water for several days, knead and wash out the starch through a cloth, then settle and dry it the same way (Grain, Flour and Bread).
- Make starch water. Mix 1 tablespoon (about 10 g) of starch to a smooth cream with a little cold water. Pour on half a litre of boiling water, stirring, until it turns clear and glassy. Thin with cold water: about 1 litre for a light finish, half that for stiff collars.
- Dip the damp, clean cloth, squeeze it out, and dry it. Iron while slightly damp.
Ironing.
- Heat the flat irons on the hearth or stove, propped on their heels so ash does not stick to the faces. Work with two: one heating, one in use.
- Clean the face by rubbing it on a cloth sprinkled with salt, then on a scrap of cloth with a little beeswax. A dirty iron marks linen.
- Judge the heat. Flick a drop of water on the face. Linen needs a hot iron: the drop dances and skitters off at once. Cotton: the drop sizzles briskly. Wool and silk need a cooler iron — the drop just hisses and steams — and a damp cloth between iron and fabric. If the iron browns a test rag, it is too hot; let it cool.
- Damp the cloth. Linen irons best slightly damp: sprinkle dry pieces with water, roll them up tightly, and leave for an hour.
- Iron with long, firm strokes along the threads, collars and cuffs first, then the large parts. Air the ironed pieces by the fire until fully dry before putting them away.
No iron? Fold sheets and table linen while damp, smooth them by hand, and press them under a board weighted with stones, or put them through the mangle. In the Viking age, linen was smoothed by rubbing it with a heavy glass or stone "slickstone" on a smooth board.
Keeping cloth clean
- Aprons, smocks and overalls over clothes for dirty work; they are easier to wash.
- Next-to-skin linen — shirts, shifts, underclothes — changed and washed often keeps outer clothes clean, which then need washing far less. For centuries this was how people kept clean.
- Brush woollen outer clothes when dry; most mud and dust falls out. Air them in the wind.
- Sponge grease spots at once with fuller's earth.
- Store clean, mended and completely dry, in a chest or closed bag, away from moths (Household Pests).
How to tell it worked
- Clean: washed cloth smells of nothing, or of fresh air; no sour, sweaty or musty smell. Squeezed in the last rinse, no suds or cloudiness come out.
- White: held next to a piece of chalk or snow in daylight, bleached linen looks nearly as white, without grey or yellow.
- Strong: bleached cloth tears no more easily than before. Pull a small piece hard between your hands: if it tears like paper, it has been over-bleached.
Note Troubleshooting. Greyish, dingy whites → soap left in, hard water scum, or too little rinsing. Rinse more, soften the water, boil whites now and then. Yellow patches → soap or lye not rinsed out, or the iron too hot. Rewash, sun-bleach. Stains set in permanently → washed in hot water before soaking cold. Next time soak first. Holes and weak, papery cloth after bleaching → lye too strong, cloth left dry in hot sun, or too much chlorine. Use weaker lye, keep cloth wet on the grass. Linen still grey after weeks on the grass → too few lye rounds between crofting, or the cloth was let dry out. Alternate properly. Wool came out small and thick → it felted: water too hot, or rubbed. It cannot be undone; use it as felt. Starch patchy and flaky → starch water too thick or not cooked clear. Thin it and boil until glassy.
Dangers
Danger Small children drown in wash tubs and buckets. A toddler who tips head-first into a tub or bucket with only a few centimetres of water cannot get out. Never leave a child alone near tubs, coppers, rinse buckets or a washing stream, and empty them as soon as you have finished.
Danger Boiling coppers and hot lye. A tipped copper of boiling water scalds a whole body. Set it firmly on a level hearth, never fill it more than three-quarters, keep children well away, and move hot water in small buckets. Lye in the eyes can blind: wash at once with plenty of clean water for 15 minutes (Lye and Potash, Emergencies).
- Mangles crush fingers: feed cloth with flat hands well back from the rollers, and never let children turn the crank while someone feeds it.
- Charcoal-filled box irons give off carbon monoxide; use them only in a well-aired room. Hot irons left face-down start fires.
- Acids: always add acid to water; a sour strong enough to sting a cut is too strong for cloth.
Warning Never mix chlorine bleach with acids, vinegar, urine or ammonia. The mixture gives off chlorine or chloramine gas, which burns the lungs and can kill in a closed washhouse. Rinse out one before using the other.
- Heavy work. Wet laundry is heavy: lift loads with a straight back, share the wringing, and use a handcart or yoke for water.
What this unlocks
Clean clothing and bedding stop lice-borne typhus and much skin disease (Personal Hygiene, Household Pests). White linen and cotton take clear dyes (Dyes and Mordants) and make white rag Paper. Clean, boiled linen makes dressings for Wound Care and Antiseptics and Basic Surgery. The demand for faster bleaching built the chemical industry: Sulfuric Acid for sours, Soda Ash and Baking Soda and Chlorine and Bleach for whitening. In time, the dolly, posser and mangle were driven by cranks and then motors — the first washing machines (The Electric Motor, Fans, Vacuum Cleaners and Washing Machines), and the flat iron became the electric iron (Electric Kettles, Irons, Heaters and Cookers).
How it was first done
Washing by pounding cloth on stones in a stream is as old as cloth itself. Ancient Egyptian tomb paintings show professional washermen beating and wringing linen. In Rome, fullers washed clothes and finished new cloth in workshops using stale urine collected from the streets; the Emperor Vespasian (AD 69–79) famously taxed the urine trade, giving rise to the saying "money does not stink". Through the Middle Ages, households "bucked" linen with ash lye a few times a year in great washes. From the 1500s the bleachers around Haarlem in the Netherlands became so famous that linen from Scotland and Ireland was shipped there to be whitened on their wide green fields, a process taking up to eight months. In 1756 the Scottish doctor Francis Home showed that dilute sulfuric acid could replace buttermilk sours, and in the 1780s and 1790s chlorine bleaches from Berthollet in France and Tennant in Scotland cut bleaching from months to days (Chlorine and Bleach). Hand mangles and ridged washboards became common household tools in the 1800s, and the first powered washing machines appeared in the early 1900s.
Source: content/entries/textiles/laundry-and-bleaching.md