◆ Rebuild

Part 8 · Chemistry

Phosphoric Acid and Phosphates

Dissolve ground phosphate rock in sulfuric acid, filter off the gypsum, and you have phosphoric acid, the mother of all phosphates. How to make it by the tonne, deal with its gypsum and fluorine, purify it for food and medicine, and turn it into strong fertilisers, baking powder, rust converter, protective coatings on steel, water treatment and detergents.

Difficulty
●●●●●
Time
An afternoon to start a barrel batch and two days to finish it; a works runs day and night
Steps from zero
35 prerequisites →

You need first

Sulfuric AcidPhosphorusChemical Fertilisers

This unlocks

—
The full path from nothing — 35 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Pottery
  10. The Kiln
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Salt
  15. Lye and Potash
  16. Fermentation
  17. The Wheel and Axle
  18. Glass
  19. Bellows
  20. Saltpeter
  21. The Lathe
  22. Copper Smelting
  23. Iron (the Bloomery)
  24. Sulfuric Acid
  25. Laboratory Glassware
  26. Blacksmithing
  27. Phosphorus
  28. The Battery
  29. Steel
  30. The Steam Engine
  31. Electrolysis
  32. Hydrogen, Oxygen and Gases
  33. Machine Tools
  34. Ammonia
  35. Chemical Fertilisers
  36. Phosphoric Acid and Phosphates

Do them roughly in this order. See it on the tech tree →

Why it matters

The Phosphorus chapter makes a little phosphoric acid from bone ash in a crock, enough for a laboratory. A growing settlement needs it by the tonne: for concentrated fertiliser, baking powder, rust-proofing steel, keeping scale out of boilers and pipes, and softening washing water.

Phosphoric acid is a clear, syrupy, sour liquid, far gentler than sulfuric or nitric acid but strong enough to dissolve rust. With lime, soda or ammonia it gives a family of phosphate salts, each with its own job. This chapter covers the industrial wet process from rock, the mountain of gypsum it leaves, cleaning the acid until it is fit to eat, and the main things made from it.

How it works

The reaction. Phosphate rock is mostly apatite, a calcium phosphate that also holds some fluoride. Sulfuric acid takes the calcium away as gypsum (calcium sulfate) and sets the phosphoric acid free:

calcium phosphate + sulfuric acid + water → phosphoric acid + gypsum

The fluoride in the rock comes off partly as hydrogen fluoride gas. This attacks the sand in the rock and forms silicon tetrafluoride, a choking gas that must be caught.

Growing good gypsum crystals. Everything in a wet-process works depends on the gypsum. Muddy gypsum clogs the filter and holds acid back; big, chunky crystals filter fast and wash clean. They grow when the slurry is kept at 70–80 °C, when acid and rock are fed gradually into a big stirred tank already full of slurry (never mixed neat), when there is always a slight excess of sulfuric acid (2–3% in the liquid), and when they have 4–8 hours to grow. At these temperatures the gypsum forms as the ordinary mineral with water in its crystals, the dihydrate. This dihydrate process is the simplest and most forgiving. It gives a "filter acid" of about 26–30% P₂O₅.

How strength is written. Phosphates are traded by their content of P₂O₅, phosphorus written as if it were its oxide, just as on fertiliser bags (Chemical Fertilisers). To turn % P₂O₅ into % phosphoric acid, multiply by 1.38. Filter acid at 28% P₂O₅ is about 39% phosphoric acid. Commercial "merchant grade" at 54% P₂O₅ is about 75%.

Three hydrogens, three families of salts. A molecule of phosphoric acid has three hydrogens that a base can replace, one after another. Replace one with sodium (or calcium, or ammonium) and you get a mono- phosphate, which is still acid. Replace two and you get a di- phosphate, which is mildly alkaline. Replace all three and you get a tri- phosphate, which is strongly alkaline. So by choosing how much base you add, you choose how acid or alkaline the product is. This is the key to every use below.

+ 1 base + 2nd base + 3rd base Phosphoric acid 3 hydrogens free pH 1–2 rust converter phosphating drinks, dental cement Mono- phosphates acid salts pH about 4–4.5 monocalcium: baking powder and triple superphosphate MAP fertiliser 11–52–0 Di- phosphates mildly alkaline pH about 8–9 DAP fertiliser 18–46–0 dicalcium: animal feed disodium: water softener Tri- phosphates strongly alkaline, pH 12 trisodium: cleaner, boiler water Base = soda, lye, lime or ammonia. Mono-, di-, tri- = how many of the three hydrogens are replaced.
Fig. 1 The phosphate ladder. Each step replaces one more hydrogen of phosphoric acid with a metal or ammonium. The first salts are acid, the last strongly alkaline, and each has its own uses.

What you need

Item For a works making 1 t of P₂O₅ a day From
Phosphate rock, ground to flour about 3.5 t a day Chemical Fertilisers, Ball Mills, Crushers and Grinders
Sulfuric acid, as 93–98% about 3 t a day Sulfuric Acid
Water 5–10 m³ a day Water Treatment for a Town
Reactor: tank 4–6 m³, with a strong stirrer Kept at 70–80 °C Rubber- or lead-lined steel, or acid brick (Firebrick and Refractories)
Filter: cloth on a perforated tray under vacuum, or a filter press Separates gypsum The Vacuum Pump; tightly woven wool or acid-proof cloth
Evaporator: lead-lined or graphite-tubed pan Concentrates the acid Heat Exchangers
Scrubber: tower packed with broken stoneware, sprayed with water Catches fluorine gases Laboratory Glassware for small rigs
Gypsum stack 5 t of wet gypsum per t of P₂O₅ Sealed clay base (Finding and Preparing Clay)

For the barrel scale (about 10 kg of rock a batch): a pitch- or lead-lined wooden barrel or a large stoneware crock, a wooden paddle, cloth filter bags, a lead or enamelled pan for boiling down (Enamel on Metal), and a site outdoors and downwind of everything.

Where to find it

  • Phosphate rock: grey, brown or black, dull, in nodules and beds in marine shale, chalk or limestone, often with fossil teeth and bones, and heavier than limestone (Chemical Fertilisers, Phosphorus). Good rock has 30–35% P₂O₅. Test any find for phosphate with molybdate (Identifying Substances).
  • Bone ash: always the cleanest raw material. It holds almost no fluorine, arsenic or cadmium, so it is the best start for food-grade acid on a small scale (Phosphorus).
  • Oak galls for tannin in rust converter: the hard round swellings on oak twigs (Ink).
  • Sand (silica), limestone and soda for the purification steps (Lime, Soda Ash and Baking Soda).

Method 1: Wet-process acid from rock

Rock flourground to 0.15 mm Sulfuric acid0.9 kg per kg rock Reactorstirred, 70–80 °C4–8 hours slurry Filter + gypsum cake strong wash 1 wash 2–3 clean water weak wash acid back to reactor Gypsum stack5 t per t P₂O₅lined base, runoff pond filter acid, 26–30% P₂O₅ Evaporatorto 40–54%P₂O₅ Scrubberwater spray catchesfluorine gasesfluosilicic acidvent gasvent gas to scrubber
Fig. 2 A dihydrate phosphoric acid works. Ground rock and sulfuric acid go into a hot stirred reactor full of slurry; the slurry is filtered and the gypsum cake washed with water that flows backwards through the washes; filter acid goes on to be concentrated. Fluorine gases from the reactor and evaporator are scrubbed with water into fluosilicic acid.
  1. Grind the rock until most passes a 0.15 mm sieve, as fine as flour (Ball Mills, Crushers and Grinders). Coarse grains get coated with gypsum before they dissolve, and their phosphate is lost.
  2. Work out the acid. Rock with 30–33% P₂O₅ needs about 0.9 kg of pure sulfuric acid per kg. Check with a 100 g trial: digest, filter and test the liquid for sulfate (Identifying Substances). You want a little free sulfate, not a lot.
  3. Prime the reactor half full with slurry from the last batch, or, the first time, with water and some ground gypsum as seed crystals. Heat to 75 °C.
  4. Feed steadily. Add rock and sulfuric acid slowly and together, at opposite sides of the stirred tank, over several hours. Feed the acid in with the weak wash acid returning from the filter, which dilutes it. The reaction's own heat holds 70–80 °C: add weak acid if it climbs, steam if it falls.
  5. Hold for 4–8 hours in all. Look at a drop under a lens (The Microscope): you want thick, separate crystals, not mud, and about one third solids.
  6. Filter and wash. Draw the slurry dry on the cloth by vacuum. The first strong liquid is filter acid, the product. Wash the cake three times: clean water for the last wash, the last wash's liquid for the one before, and the first wash's weak acid back to the reactor. This counter-current washing recovers 95% or more of the phosphate while adding little water.
  7. Concentrate in a lead-lined or graphite-tubed evaporator to 40–54% P₂O₅, best under vacuum at 80–90 °C. More fluorine gas comes off; send it to the scrubber.
  8. Settle for several days in a lined tank. Fine gypsum and iron and aluminium salts drop as sludge. The clear, dark green-brown acid above is merchant-grade acid for fertiliser.

The barrel version. Outdoors, put 20 litres of weak acid or water in the lined barrel. Stir in 10 kg of rock flour and about 9 kg of concentrated sulfuric acid in small, alternating portions over two to three hours, standing upwind. The acid heats the water; if it starts to boil, pause. Cover loosely and stir now and then for one to two days while it stays warm. Then filter through cloth bags, wash as above, and boil down in a lead or enamelled pan. Expect 25–30 litres of weak acid, which boils down to about 6 litres (8 kg) of 50% acid.

The scrubber and fluosilicic acid

Lead every vent from the reactor and the evaporator up a short tower packed with broken stoneware, with water trickling down over it. The fluorine gases dissolve to make fluosilicic acid, and some sand-like silica forms in the tower. At 15–25% strength it is a useful product. It fluoridates drinking water at about 1 milligram of fluoride per litre (Water Treatment for a Town, Fluorspar and Fluorine Compounds). With soda it gives sodium fluosilicate, used for enamels and as a timber preservative. Never let the vent gases out unwashed: they burn the lungs and kill vegetation and grazing animals downwind.

Gypsum by-product

Every tonne of P₂O₅ leaves about 5 tonnes of damp phosphogypsum. It is the biggest headache of the industry.

  • Stack it on a base of rammed clay, sloped to a lined pond that catches rain running off. The runoff is acid and full of phosphate and fluoride: return it to the works as process water, never to a stream.
  • Neutralise the surface with limestone or slaked lime where people or animals go near.
  • What it is good for, once washed and neutralised: a soil conditioner that loosens salty, sticky clay soils and adds sulfur (Understanding Soil); a set retarder for Portland Cement (3–5%); and, after washing and calcining, plaster (Gypsum and Plaster of Paris).
  • Its hidden danger. Phosphate rock contains a little uranium, and the gypsum keeps its decay product radium, which gives off radon gas (Detecting Radiation). Do not build houses on gypsum stacks or make house plaster from rock-derived gypsum without testing it. Gypsum from bone ash has no such problem.

Method 2: Purifying the acid

Merchant acid is fine for fertiliser. For food, medicine and laboratory use it carries too much sulfate, fluoride, iron, aluminium, arsenic, cadmium and coloured organic matter. Clean it in steps, testing after each (Identifying Substances):

  1. Remove sulfate. Stir in a little extra ground rock or slaked lime, a few grams at a time. More gypsum forms and settles. Stop when a drop of barium chloride solution added to a diluted sample gives no white cloud.
  2. Remove fluoride. Add finely ground sand and a small amount of soda (Soda Ash and Baking Soda) and keep it warm for a few hours. Fluoride is caught as sodium fluosilicate, a white, gritty solid. Filter. Boiling the acid hard during concentration also drives off much of the fluoride.
  3. Remove arsenic and heavy metals. Dilute to about 30% and stir in a little sodium sulfide solution, made by fusing Sulfur with soda. Arsenic, lead and copper settle as dark or yellow sulfides. This step gives off hydrogen sulfide (see Dangers). Do it outdoors, then blow air through the acid to clear the gas, and filter.
  4. Remove colour. Warm with 1–2% activated charcoal (Activated Charcoal) for an hour and filter.
  5. Solvent extraction (works scale, in outline). Shake the acid with an alcohol that does not mix with water, such as butanol or amyl alcohol from fusel oil (Distillation, Ether, Acetone and Solvents). The phosphoric acid moves into the alcohol; iron, aluminium, calcium and most metals stay behind in the water. Separate the layers, wash the alcohol layer with a little clean water, then shake it with plenty of water, which takes the acid back. Boil off the remaining solvent and recover it. This gives acid nearly as pure as the furnace kind. It is the same separation used to win copper from dirty leach liquors (Leaching, Solvent Extraction and Electrowinning).
  6. Concentrate to 75–85% in glass, enamel or graphite. Food-grade acid is water-white, has no smell, and contains no more than a few parts per million of arsenic and heavy metals.

Furnace acid. The other road to pure acid is to make the element first (Phosphorus, Electric Kilns and Furnaces), burn it in dry air to white phosphorus pentoxide smoke, and absorb the smoke in water. The acid is very pure except for a trace of arsenic, which step 3 removes. It costs much more energy. Use it if you already make phosphorus for matches.

Checking strength. Weigh exactly 100 mL in a measuring flask. 168–169 g means about 85% acid; 157–158 g, 75%; 133 g, 50%; 118 g, 30%.

Phosphates and their uses

Fertilisers

  • Triple superphosphate (about 0–46–0). Mix ground phosphate rock with 1.3–1.5 kg of 50%-P₂O₅ acid per kg of rock in a lined trough, as for ordinary superphosphate (Chemical Fertilisers). It sets into a porous mass. Cure it in a heap for 3–6 weeks and crush it. It has more than twice the strength of ordinary superphosphate and no gypsum to carry, so it is cheaper to haul.
  • Ammonium phosphates. Run ammonia gas or strong ammonia water (Ammonia) into the acid. With one part ammonia to one part acid (by chemical units, ending at about pH 4–4.5) you get monoammonium phosphate (MAP), about 11–52–0. With twice as much ammonia (pH about 8) you get diammonium phosphate (DAP), about 18–46–0. Dry and granulate. These carry two nutrients in one, are the strongest common fertilisers, and also make good fire retardants (Firefighting).
  • Feed phosphate. Neutralise defluorinated acid (purification step 2) with slaked lime to about pH 5–6. White dicalcium phosphate settles out. Livestock short of phosphorus chew bones and wood and grow poorly; about 50 g a day in the feed of a cow on poor pasture is a usual dose, a few grams for a sheep or goat (Animal Health). Never feed phosphate made from rock without defluorinating it: fluoride cripples the bones and teeth of grazing animals.

Baking powder

A phosphate baking powder raises dough with gas made when the powder is wetted and again in the oven. It contains no tartar from wine, so it can be made anywhere. It works alongside the cream-of-tartar powders in Citric and Tartaric Acid.

  1. Make monocalcium phosphate. Use food-grade acid only (Method 2). For every 100 g of 75% acid, sift in 28 g of slaked lime (Lime), a little at a time, stirring. It gets hot and turns into a stiff white paste. Spread it thinly and dry it at 50–60 °C. Grind it fine.
  2. Mix. By weight: 30 parts baking soda (sodium bicarbonate, Soda Ash and Baking Soda), 38 parts monocalcium phosphate, 32 parts dry starch (maize or potato, dried in a warm oven). The starch keeps the two actives apart and soaks up damp.
  3. Store in a dry, tightly closed tin. Use 4–5 g (one level teaspoon) per 100–125 g of flour.

Test it: a teaspoon in half a glass of warm water should fizz hard at once, and a little more when you heat it. Weak fizz means it took up damp. A soapy or bitter taste in the bread means too much soda; increase the phosphate slightly.

Rust converter

Rust converter turns loose red rust into a tight, dark layer of iron phosphate that paint grips and that slows further rust. It is the bridge between a rusty gate and a painted one when you cannot get the metal bright.

Paint on rust Paint on converted rust Paint blistered Rust swells under the paint cracked: water gets in Loose red rust porous and flaky steel Dark iron phosphate thin, tight, holds paint Paint grips and stays sealed steel
Fig. 3 What rust converter does. Untreated, red rust is loose and porous; paint on it lifts off as rust grows underneath. Phosphoric acid turns the rust and the metal surface into a thin, tight layer of dark iron phosphate that paint sticks to.
  1. Recipe for 1 litre: 200 mL of 75% phosphoric acid, 50 g of tannin (boil 100 g of crushed oak galls in 500 mL of water for an hour and strain, Ink), a teaspoon of wetting agent (a little soap solution or Turkey red oil, Detergents and Wetting Agents) and water to make 1 litre. The tannin turns the layer blacker and tighter. Without it, plain 15–20% acid still works.
  2. Prepare: knock off loose flakes and scale with a wire brush (Brooms, Brushes and Combs). Leave the tight rust. Wipe off oil and grease with paraffin or soda water.
  3. Apply with a brush, thinly, working it into pits. One litre covers about 8–10 m².
  4. Wait 24 hours. The red-brown turns blue-black to grey-black. Where red still shows, put on a second coat.
  5. Wipe off any white powder with a damp cloth and let it dry. Paint within two days (Pigments, Paints and Varnish), before damp starts new rust through the thin layer.

Good versus bad: a good job is evenly dark, hard and dry to the touch, and a fingernail does not scrape off red powder. A bad one stays sticky (too much acid left; wipe and rinse lightly) or shows red patches (rust too thick or the coat too thin).

Phosphating bath

New steel can be given a grey crystalline phosphate coat that holds oil or paint and resists rust far better than bare metal. It is called phosphating or Parkerising. Tools, bolts, sheet steel before painting, and parts of machines that rub are treated this way (Corrosion and Its Prevention, Sheet Metal and Rolling).

  1. The bath, in outline: a stainless, enamelled or stoneware tank of water holding about 2% phosphoric acid, with zinc oxide or manganese carbonate dissolved in it (roughly 5 g per litre to start). Add a pad of clean steel wool and simmer for an hour to season it: the bath needs a little dissolved iron before it coats well.
  2. Clean the parts completely: boil in strong soda water to degrease, then sandblast or pickle in dilute acid to bare grey metal (Abrasives and Grinding Stones). Rinse.
  3. Immerse at 90–95 °C, just under the boil. Fine bubbles stream off the steel. After 10–30 minutes the bubbling stops. That is the sign the coat is complete.
  4. Rinse, dry in warm air, and at once oil the parts or paint them. Zinc phosphate is light grey and suits paint. Manganese phosphate is dark grey to black, holds oil best, and is used for parts that rub.

Water treatment

  • Scale prevention. Heat sodium phosphate to make polyphosphate glass (see Detergents and Wetting Agents). A dose of only 1–5 milligrams per litre of water stops lime scale forming in pipes, kettles and hot-water systems (Hot Water and Central Heating). It works even though there is far too little to bind all the calcium.
  • Boiler water. Keeping 20–50 mg/L of trisodium phosphate in a boiler turns calcium into a soft sludge that blows down, instead of hard scale on the tubes.
  • Old lead pipes. About 1 mg/L of phosphate (as phosphorus) in town water builds a thin phosphate skin inside lead pipes and cuts the lead people drink (Pipes, Plumbing and Aqueducts, Lead).

Detergents, food and medicine

How to tell it worked

  • Acid: syrupy, sour, no fumes. Neutralised with soda, it gives a yellow precipitate with silver nitrate (Identifying Substances).
  • Yield: 90–95% of the rock's P₂O₅ in the acid. Washed gypsum holding over 1% P₂O₅ (molybdate test) means coarse rock or short washing.
  • Gypsum: filters in minutes, not hours; the washed cake is off-white and only faintly sour.
  • Fertiliser: a strip trial (Chemical Fertilisers).
  • Rust converter and phosphating: paint a treated and an untreated steel strip, scratch both through to the metal, and hang them outdoors. After a month the treated one shows little or no rust creeping from the scratch.

Note Troubleshooting Filter clogs, gypsum like mud → temperature too low or swinging, acid and rock added too fast or in one place, or not enough seed slurry. Feed slower into more slurry; hold 75 °C. Rock grains coated, low yield → rock too coarse, or too little free sulfuric acid; grind finer and raise the acid slightly. Too much sulfate in the acid → too much sulfuric acid; reduce the feed and desulfate with a little rock. Acid green-black and full of sediment → normal for merchant acid; settle longer, or purify. Baking powder lumpy and weak → it took up damp; dry the starch better and keep the tin closed. Phosphate coat patchy or powdery → part not fully cleaned, or bath too cold, too weak or not seasoned.

Dangers

Danger Fluorine gases. Phosphate rock in hot acid gives off hydrogen fluoride and silicon tetrafluoride. They burn the eyes and lungs, sometimes with the full harm showing only hours later, and they poison livestock and crops downwind. Work rock only outdoors or with a working scrubber, stand upwind, and keep animals off land near the works. Read Fluorspar and Fluorine Compounds for first aid with fluoride burns.

Danger Hydrogen sulfide. Purifying with sodium sulfide releases a gas that smells of rotten eggs at first. At dangerous strength it deadens the sense of smell, so you stop noticing it just as it becomes deadly, and a few breaths can kill. Do it only outdoors, never in a pit or tank, with a second person watching from upwind.

  • Sulfuric acid: everything in Sulfuric Acid applies. Always add acid to water, never water to acid. Wear eye protection, gloves and an apron.
  • Phosphoric acid burns less than sulfuric acid, but it still harms eyes and skin. Hot concentrated acid causes deep burns. Wash at once with plenty of water.
  • Never use fertiliser-grade acid for food. Acid made from rock carries arsenic, cadmium, fluoride and a little uranium. Only bone-ash or purified acid goes into food or medicine.
  • Radioactive gypsum: see the gypsum section.
  • Water pollution. Phosphate runoff from stacks, fields and laundries feeds algae that choke lakes and kill fish (Phosphorus).

What this unlocks

Concentrated fertilisers that travel cheaply feed growing towns (Chemical Fertilisers, The Great Staple Crops). Phosphate baking powder makes quick breads and cakes (Grain, Flour and Bread). Rust converter and phosphating keep Sheet Metal and Rolling roofs, Tins, Cans, Drums and Tanks, tools and the bodies of the The Motor Vehicle painted and sound. Scale-free Boilers and Pressure Vessels and pipes, softer washing water (Detergents and Wetting Agents), fluoridated drinking water (Water Treatment for a Town), phosphate buffers for the The Medical Laboratory, dental cement, the electrolyte of phosphoric-acid Fuel Cells, and fire-retardant salts all come from the same tank of acid. The fluosilicic acid and gypsum, handled with care, become useful products rather than waste.

How it was first done

Phosphoric acid was known to chemists of the 1700s, who made it from bone ash and from burning phosphorus. Justus von Liebig showed in 1840 that bones treated with sulfuric acid feed plants faster, and John Bennet Lawes began making superphosphate from rock in England in 1842. In the United States the Harvard chemist Eben Horsford patented an acid calcium phosphate as a replacement for yeast in 1856. The Rumford Chemical Works sold it as phosphate baking powder in the 1860s.

The wet process grew in Germany and the United States in the late 1800s and early 1900s. Continuous dihydrate plants with counter-current washing were developed in the 1910s–1930s, notably by the Dorr Company in America. In the same period electric-furnace phosphorus made pure furnace acid for food. Thomas Coslett in Britain patented phosphate coating of iron in 1906. The American Parker company improved it from about 1915, and its name, Parkerising, stuck. In the 1960s and 70s, polyphosphate detergents were found to be choking lakes, and many countries limited them.

Source: content/entries/chemistry/phosphoric-acid.md