◆ Rebuild

Part 3 · Metals

Platinum and the Platinum Metals

A heavy grey metal from a few gold-bearing rivers that no fire can tarnish and no single acid can dissolve. It melts at 1,768 °C, far above any early furnace, so it was first made workable as a powder, pressed and hammered hot. Dissolved in aqua regia, thrown down as a yellow salt and turned into sponge, it becomes crucibles, wire, furnace thermocouples, electrodes and the catalyst gauzes that make nitric acid.

Difficulty
●●●●●
Time
Weeks of panning for a few grams; two to four days from crude grains to a sponge; a day to press and forge an ingot; a day for each crucible or few metres of wire
Steps from zero
24 prerequisites →

You need first

Gold and SilverNitric AcidHydrochloric Acid

This unlocks

Fuel CellsPalladium, Rhodium and Iridium
The full path from nothing — 24 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Lime
  14. Salt
  15. Lye and Potash
  16. Glass
  17. Bellows
  18. Saltpeter
  19. Copper Smelting
  20. Lead
  21. Sulfuric Acid
  22. Gold and Silver
  23. Nitric Acid
  24. Hydrochloric Acid
  25. Platinum and the Platinum Metals

Do them roughly in this order. See it on the tech tree →

Why it matters

Platinum does what no other metal you can make will do. It never tarnishes, even red-hot in air. No single acid dissolves it, nor do most molten salts. It melts at 1,768 °C, so it survives any kiln. And it expands with heat almost exactly as soft glass does, so it seals through glass (The Light Bulb).

So a few grams of it give you:

It is rare: a good platinum river gives a hard-working crew a few grams a day. Never throw away a scrap or filing; platinum is recycled forever.

How it works

The platinum metals come together. Natural platinum is never pure. Its grains carry iron (5–15%), a little copper and gold, and the five sister metals: palladium, rhodium, iridium, osmium and ruthenium. Iridium and osmium also form separate, very hard, flat grains called osmiridium.

Aqua regia dissolves it. Nitric or hydrochloric acid alone cannot touch platinum. Mixed (1 part nitric to 3 of hydrochloric), they turn it into chloroplatinic acid, an orange-red liquid. Osmiridium is left behind.

Sal ammoniac throws it down. Add ammonium chloride (sal ammoniac) to the platinum solution and a lemon-yellow crystalline salt falls out: ammonium chloroplatinate. It hardly dissolves in water containing sal ammoniac, so nearly all the platinum comes down, while iron, copper, palladium and most rhodium stay dissolved. That one step is the secret of refining.

Heat makes sponge. Heated, the yellow salt gives off its ammonia and chlorine as gases and leaves a grey, spongy cake of pure platinum sponge, 44% of the salt's weight.

The sponge welds without melting. Because platinum makes no oxide skin, clean grains pressed hard together and heated white-hot weld into solid metal. William Hyde Wollaston used this, around 1800–1805, to make the first truly malleable platinum with no furnace hotter than a smith's. Melting it whole needs an oxy-hydrogen flame or an induction furnace (Very-High-Temperature Furnaces).

What you need

Item Amount or size See
Crude platinum grains 50–500 g for a useful batch Below
Strong Nitric Acid and Hydrochloric Acid About 4–5 ml of mixed aqua regia per gram of crude platinum, more as it is used up
Sal ammoniac About 1 g per gram of platinum Ammonia or natural crusts round volcanic vents
Green vitriol A few grams per batch To remove gold (Gold and Silver)
Porcelain or glass dishes, sand bath, filters; wooden bowl and pestle Dissolving; grinding sponge Laboratory Glassware
Press barrel and plunger, lever or screw press Compressing sponge Below
Smith's forge reaching white heat, anvil, hammers Welding the ingot Blacksmithing
Small rolling mill and draw plate Sheet and wire Sheet Metal and Rolling, Iron and Brass Wire

Where to find it

  • Placer platinum. Small, steel-grey to silver-white grains and flattened scales, 0.1–2 mm, sometimes nuggets, that stay in the gold pan with the gold (Gold and Silver). Dull beside gold and about as heavy, it does not tarnish when heated red and is often weakly magnetic because of its iron. Found in rivers draining dark green to black serpentinite rich in chromite — in the Urals, the Chocó of Colombia, British Columbia, Ethiopia and Alaska.
  • Osmiridium: tiny, very hard, bright, tin-white, flat six-sided flakes among the platinum grains. A steel needle will not scratch them.
  • From nickel and copper refining. Nickel–copper sulfide ores (Nickel and Cobalt) carry traces of platinum and palladium, which gather with gold and silver in the anode slime of the refining tanks (Electrolysis). Save every slime.

Test a grain. Put a suspect grain in a few drops of hot nitric acid: nothing happens. Add three times as much hydrochloric acid and warm it for an hour: it slowly dissolves and the drop turns yellow to orange. Add a crystal of sal ammoniac: a yellow speck of fine crystals forms. Gold also dissolves, but gives no yellow salt with sal ammoniac.

Step 1: Dissolving the crude platinum

1 Aqua regiawarm, outdoors, days 2 Filterosmiridium stays behind 3 Green vitriolgold falls out 4 Sal ammoniacyellow salt falls 5 Ignitered heat: grey sponge 6 Grind gentlywooden bowl; wash fine 7 Press wetbarrel and lever 8 White heat, hammerwelds into an ingot
Fig. 1 Wollaston's route. Crude grains dissolve in aqua regia, leaving osmiridium; gold is thrown down with green vitriol; sal ammoniac precipitates yellow ammonium chloroplatinate; heating gives sponge, which is ground, pressed wet in a barrel, heated white and hammered into a solid ingot.
  1. Clean the grains. Pan down to platinum and gold. Lift magnetite with a weak magnet (re-pan what it lifts: iron-rich platinum is slightly magnetic). Boil in hydrochloric acid for an hour to dissolve iron coatings.
  2. Dissolve. Put the grains in a glazed porcelain or glass dish on a warm sand bath, outdoors, and cover with aqua regia freshly mixed (3 volumes strong hydrochloric, 1 volume strong nitric acid). Wollaston diluted it with an equal volume of water, which is slower but leaves more iridium undissolved. Keep it just below boiling, adding fresh acid as it is spent. A large batch takes two to four days.
  3. Pour off and filter the orange-red liquid through glass wool or a sand filter. What stays is black sand and osmiridium: wash and keep it (for pen-nib tips, below).
  4. Drive off the nitric acid. Evaporate the liquid nearly to a syrup, add a little strong hydrochloric acid, evaporate again, and repeat two or three times, until no brown fumes come off. Left-over nitric acid spoils the next step.
  5. Dilute the syrup with five to ten times its volume of water. It is now chloroplatinic acid with gold, iron, copper and the other platinum metals.
  6. Remove gold. Stir in a solution of green vitriol (ferrous sulfate) a little at a time. Gold falls as a brown powder; platinum stays dissolved. Let it settle for a day, filter, and save the gold (Gold and Silver).

Step 2: The yellow salt and the sponge

  1. Precipitate. Stir into the clear liquid a strong, filtered solution of sal ammoniac in water (about 1 g of sal ammoniac per gram of platinum, plus some extra). A heavy, lemon-yellow crystalline powder falls. If it is orange or brick-red, iridium came down with it: the platinum will be harder and stiffer, good for crucibles but not for thermocouples.
  2. Settle for a day. Pour off the liquid and keep it: it holds palladium, rhodium and some platinum. Iron or zinc strips hung in it for a week throw down a black mud of these metals; store it. Separating palladium, rhodium, iridium, osmium and ruthenium from it is the subject of Palladium, Rhodium and Iridium.
  3. Wash the salt three or four times with water containing a little sal ammoniac (pure water dissolves some), and dry it.
  4. Ignite. Put the dry salt in a covered fireclay or porcelain crucible and heat it slowly: first gently, at about 300–400 °C (no visible glow), until white fumes stop, then to a bright red for 20–30 minutes. Do this outdoors; the fumes are choking.
  5. Sponge. A grey, porous cake remains, 44% of the salt's weight. A yellow core means it needs more heat.

Step 3: Wollaston's powder method

  1. Grind gently. Rub the sponge between the palms, then in a wooden bowl with a wooden pestle. Never use an iron mortar or press hard: burnished, flattened grains will not weld.
  2. Wash and grade. Stir the powder into water, let it settle a few seconds, and pour the cloudy water with the finest grains into a second bowl. The finest mud makes the best metal; regrind the coarse part.
  3. The press barrel. A brass or steel tube about 17–18 cm long, 3 cm bore, very slightly wider at one end so that the cake slides out, with a steel plunger that fits closely and a steel stopper for the narrow end. Oil the inside lightly and line it with a strip of paper.
  4. Fill and press wet. Fill the barrel with the wet mud, let the water drain through a cloth at the bottom, and press with a lever or screw press — Wollaston used a long iron lever — as hard as the plunger will bear. The cake comes out firm, like dense chalk.
  5. Dry and heat. Dry the cake slowly over charcoal, bring it to red heat to drive off grease and water, then hold it at a white heat (1,300–1,500 °C, too bright to look at long) in the hottest part of a forge or wind furnace for 20 minutes.
  6. Hammer hot. Stand the white-hot cake on end on the anvil and strike the end a few heavy blows; reheat and repeat. The grains weld into a dense, ringing ingot.
  7. Forge it like soft iron into a bar. Platinum forms no scale, and two pieces hammered together at white heat weld with no flux.

The other route is to melt sponge in a lime block with an oxy-hydrogen or oxy-gas flame (Very-High-Temperature Furnaces, Hydrogen, Oxygen and Gases), or in a zirconia crucible in an induction furnace (Zircon and Zirconium, Electric Kilns and Furnaces). Melting also burns off osmium and some impurities.

Platinum sheet and wire

Platinum is as soft and ductile as gold. Anneal it at a bright red (about 1,000 °C) in a clean gas or spirit flame whenever it gets stiff; it needs no pickling.

  • Sheet: roll the forged bar between polished steel rolls (Sheet Metal and Rolling) down to 0.1–0.3 mm, annealing every few passes.
  • Wire: hammer or roll a strip square, round off the corners, and draw it through a steel draw plate, then through holes in ruby or diamond for fine sizes (Iron and Brass Wire, Synthetic Gems, Industrial Diamond and Hard Abrasives). Pure platinum draws easily to 0.05 mm. 1 g of platinum gives about 24 cm of 0.5 mm wire, 1.5 m of 0.2 mm wire, or 12 m of 0.07 mm wire.
  • Very fine wire (Wollaston wire): draw a platinum wire inside a thick silver tube, as one rod, down to 0.05 mm; then dissolve the silver off in warm Nitric Acid. The platinum core left can be finer than a thousandth of a millimetre, for sensitive hot-wire instruments (High-Vacuum Pumps and Gauges).
  • Harder alloy: melt platinum with 5–10% iridium for crucibles, contacts and springs that must keep their shape.

The platinum crucible

Crucible Thermocouple Gauze 3.5 cm across Lid with handle Pipeclay triangle Wall 0.2–0.3 mm 3.5 cm tall; 25–30 ml, 20–30 g blue flame only; never melt metals in it Terminal head Closed-end porcelain sheath Pure platinum 0.35–0.5 mm Platinum + 10% rhodium Twin-bore insulating tube Fused bead the hot junction Flat pad: catalyst 0.06–0.08 mm wire, about 30 wires per cm each way Rolled: electrode 2–3 cm across, 4–5 cm tall
Fig. 2 Three platinum objects. Left, a 30 ml crucible and lid with its sizes, standing on a pipeclay triangle. Middle, a platinum thermocouple in a twin-bore porcelain tube inside a closed-end sheath. Right, platinum gauze woven from fine wire, rolled into a cylinder electrode or laid flat as a catalyst pad.

A small laboratory crucible holds 25–30 ml: about 3.5 cm across the top, 3.5 cm tall, walls 0.2–0.3 mm, weighing 20–30 g with its lid.

  1. Cut a disc of annealed sheet 8–9 cm across (8.5 cm of 0.2 mm sheet weighs about 24 g).
  2. Raise it in three or four stages over a smooth hardwood or steel form, with a horn or boxwood mallet, or spin it on a lathe over a boxwood chuck (Metal Spinning and Raising). Anneal between stages.
  3. Trim the rim and roll it into a small bead for stiffness. Make a lid, a shallow dish 4 cm across with a folded-up handle. Burnish and anneal.

Rules for using it. A platinum crucible lasts a lifetime if you follow these; break them once and it has a hole.

  • Never melt metals in it, and never heat it with anything that might be reduced to metal: lead, tin, zinc, bismuth, antimony, arsenic and silver alloy with platinum and melt straight through it.
  • Never use a smoky or yellow flame or let it touch glowing charcoal: carbon and silicon soak in and make it brittle. Use the blue part of the flame only, or an electric muffle.
  • No phosphates, sulfides or arsenic with a reducing agent, and no fusions with caustic soda or potash, nitre or peroxide: use iron, nickel or silver crucibles for those.
  • Set it on a pipeclay or silica triangle, not bare iron wire, and handle it with platinum-tipped tongs.
  • Clean it by melting potassium bisulfate in it and pouring out, or by rubbing with fine moist sea sand on a fingertip. Never scrape with steel.

Good versus bad. A good crucible is bright, smooth and evenly thick, and weighs the same (to a tenth of a milligram on an analytical balance) after a firing to red heat as before. A grey, frosted or crazed surface means carbon or silicon has got in; a bulge or dark spot is the start of a hole.

The platinum thermocouple

Platinum against platinum with 10% rhodium (the type S couple) is the standard for kilns, glass and steel furnaces up to 1,450–1,500 °C, and stays true for years. How thermocouples work and how to calibrate and read them is in Thermocouples and Thermoelectricity; here is the platinum one.

  1. Wires. Two wires, 0.35–0.5 mm across and as long as the hot part of the furnace wall plus 10–20 cm: one of pure platinum, one of platinum with 10% rhodium, melted together in a lime block or induction furnace and drawn. A 0.5 m pair of 0.5 mm wires uses about 4 g of metal.
  2. Junction. Twist the ends together for 3 mm and fuse them into a small bead in an oxy-gas flame, or by touching them to a carbon rod with a few volts and amperes.
  3. Insulate. Thread the wires through a twin-bore tube of porcelain or alumina (Alum and Alumina) inside a closed-end sheath 8–12 mm across, which keeps furnace gases, carbon, silica and metal vapours off the wires.
  4. Join to leads at the cool end, in a small terminal head kept as cool as possible.
  5. Read. It gives about 4.2 millivolts at 500 °C, 9.6 mV at 1,000 °C, 12.0 mV at 1,200 °C and 14.4 mV at 1,400 °C, with the cold ends at 0 °C. Calibrate it by melting short pieces of pure silver (962 °C) and gold (1,064 °C) wire bridged across the junction.
  6. Anneal a new or used couple by passing a current through it in air until it glows bright yellow (about 1,400 °C) for a few minutes. This removes strains that give false readings.

If you have no rhodium (it is only 0.5–2% of crude platinum and hard to separate), a couple of pure platinum against platinum with 10% iridium works, but drifts as the iridium slowly evaporates at high heat. Check it often against melting points.

Platinum gauze, electrodes and catalysts

Gauze. Draw wire to 0.06–0.08 mm and weave it on a small loom (The Loom) in plain weave with about 30 wires per centimetre each way (some 1,000 openings per square centimetre). Anneal it lightly so it lies flat.

  • Catalyst gauze: several layers stretched across the gas stream, heated red by the reaction itself, burn ammonia and air to nitric oxide at 850–900 °C, the heart of nitric acid making from Ammonia (the Ostwald process, Nitric Acid). Gauzes of platinum with 10% rhodium last much longer.
  • Gauze electrodes: rolled into a cylinder 2–3 cm across and 4–5 cm tall on a stiff platinum stem, a gauze cathode collects copper evenly when you find a sample's copper content by electrolysis and weighing (Analytical Instruments).

Platinum electrodes. A square of foil 1 × 1 cm welded (by hammering at white heat) to a 0.3 mm platinum wire; the wire sealed through the end of a soft-glass tube (Scientific Glassblowing and Glass-to-Metal Seals); a drop of mercury or a copper wire inside the tube makes contact. Nothing in ordinary electrolysis attacks it.

Platinum black. A velvety black coat of extremely fine platinum, with an enormous surface. To make it (platinising), dissolve sponge in aqua regia, drive off the nitric acid as above, and make a 2–3% solution of chloroplatinic acid with a pinch (about 0.02%) of lead acetate. Make the electrode the negative pole, with a platinum wire as positive, and pass about 30 milliamperes per square centimetre for 5–10 minutes, reversing the current every half minute. The bright metal turns soft black. Rinse it well and keep it wet. Platinised electrodes are used for conductivity cells (Water Softening and Ion Exchange), the hydrogen electrode (pH, Indicators and Buffers) and Fuel Cells.

Platinised pumice. Soak pea-sized grains of pumice or porous fired alumina in chloroplatinic acid (enough to leave about 1% platinum by weight), dry, and heat to red in a stream of hydrogen or simply in a flame. It is a catalyst bed for turning sulfur dioxide into strong Sulfuric Acid (the contact process) and for burning hydrogen out of gas streams. Johann Döbereiner's lighter of 1823 played a jet of hydrogen on platinum sponge, which glowed and lit it.

Osmiridium grains from Step 1, soldered to the tips of gold pen nibs, give a writing point that never wears (Pens, Nibs and Writing Instruments).

How to tell it worked

  • Grains dissolve only in aqua regia; the solution gives a yellow salt with sal ammoniac.
  • Salt is lemon-yellow; ignited, it leaves 44% of its weight as grey sponge.
  • Ingot rings when struck, bends without cracking, and stays bright when heated red in a clean flame and cooled.
  • Weight: platinum is 21.4 times as heavy as water, heavier than gold (19.3).
  • Thermocouple: reads 1,064 °C when gold melts at its tip.

Note Troubleshooting. Grains will not dissolve → acid weak or exhausted, or they are osmiridium. Use fresh, warm acid; osmiridium never dissolves. Little or no yellow salt → nitric acid not driven off, or solution too dilute. Evaporate again with hydrochloric acid; use more sal ammoniac. Salt orange or red → iridium. Redissolve and reprecipitate, or keep it for hard alloy. Pressed cake crumbles in the forge → powder too coarse or burnished, or not hot enough. Regrade the mud; heat to full white. Ingot cracks when forged → iron, lead or silicon left in it. Redissolve and refine, or melt it with oxygen. Crucible grey and brittle → heated in a smoky flame or on charcoal. Melt it down and remake it.

Dangers

Danger Aqua regia and its fumes. The brown and yellow gases are nitrogen oxides and chlorine, which can flood the lungs hours after you breathe them. Dissolve only outdoors, upwind, never indoors; mix the acid fresh and never store it in a closed bottle, which can burst (Nitric Acid).

Danger Osmium tetroxide. Heating osmiridium in air or boiling it with oxidising acids gives off a vapour that smells sharp, like chlorine, and stains and blinds the eyes and burns the lungs at tiny amounts. Never roast osmiridium or heat it in acid outside a strong draught. A black stain on paper held over a vessel warns that it is coming off.

  • Platinum salt allergy. Chloroplatinates cause asthma, sneezing and skin rashes that come back with every later exposure, and get worse. Wear gloves, handle salts damp, never breathe the dust.
  • Hydrogen and spirit vapour catch fire on platinum sponge and platinum black without a flame. Keep them apart.
  • Ignition fumes of the yellow salt are ammonium chloride and hydrogen chloride: choking. Outdoors.
  • White heat and hammering: eye protection and leather apron as in Blacksmithing.

What this unlocks

Analysis by weight with crucibles and gauze electrodes (Identifying Substances, Analytical Instruments); furnace control to a few degrees (Thermocouples and Thermoelectricity, Pyrometric Cones and Kiln Temperature, Steel, Glass); nitric acid from ammonia and strong sulfuric acid by the contact process (Nitric Acid, Sulfuric Acid); glass-sealed electrodes for lamps, valves and X-ray tubes (The Light Bulb, The Vacuum Tube, X-Rays); platinum prints (Platinum, Salt and Iron-Salt Prints); hot-wire vacuum gauges (High-Vacuum Pumps and Gauges); and the platinised electrodes of Fuel Cells. Later, platinum and palladium catalysts refine petrol and clean car exhausts (Petroleum and Refining, The Motor Vehicle).

How it was first done

Metalworkers of the La Tolita culture on the Pacific coast of what is now Ecuador and Colombia, about 2,000 years ago, heated platinum grains with gold dust and hammered them into tiny ornaments: platinum's first working, by a kind of sintering. Spanish miners in Colombia called the grains platina, "little silver", and threw them back into the rivers as a nuisance in the gold. The Spanish officer Antonio de Ulloa described it in 1748; samples reached England through Charles Wood and William Brownrigg about 1750.

For half a century nobody could make it malleable. Pierre-François Chabaneau in Spain managed it in the 1780s, with great labour. In London in 1800, William Hyde Wollaston and Smithson Tennant went into partnership to refine it. In the liquors left behind Wollaston found palladium (1802) and rhodium (1804), and Tennant found osmium and iridium (1803–1804). Wollaston's powder method made him rich; he described it only in his Bakerian Lecture of 1828, shortly before he died. Ruthenium was found by Karl Klaus in Kazan in 1844, from Ural platinum. In 1857 Henri Sainte-Claire Deville and Jules Debray in Paris melted platinum by the kilogram in lime blocks with oxygen and coal gas. Henri Le Chatelier introduced the platinum–rhodium thermocouple in 1886, and Wilhelm Ostwald patented burning ammonia over platinum to make nitric acid in 1902.

Source: content/entries/metals/platinum.md