◆ Rebuild

Part 2 · Earth and Fire

Bottles, Drinking Glasses and Glassware

The everyday glass and clay vessels that hold and serve drink and food — free-blown and mould-blown bottles with necks finished for corks and caps, tumblers and stemmed wine glasses, carafes and decanters with ground stoppers, pressed glass, and clay storage jars and amphorae — and how to anneal glass so it does not crack.

Difficulty
●●●●●
Time
Months of practice before blowing even bottles; then a skilled blower and a helper make 100–200 bottles or 200–400 tumblers in a day; a pressed tumbler takes under a minute; a clay storage jar takes a day to throw and a week to dry and fire
Steps from zero
7 prerequisites →

You need first

GlassPottery

This unlocks

—
The full path from nothing — 7 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Pottery
  5. Lime
  6. Lye and Potash
  7. Glass
  8. Bottles, Drinking Glasses and Glassware

Do them roughly in this order. See it on the tech tree →

Why it matters

Glass is clear, tasteless, does not rot, rust or soak anything up, and can be boiled clean. A glass bottle keeps wine, vinegar, oil, medicine and acid for years (Beer, Wine and Cider, Making Medicines), and can be washed and refilled fifty times. A drinking glass shows dirt that a clay cup hides.

Glass teaches you to melt, gather, blow and anneal glass. This chapter turns that skill into particular objects with their own sizes and tricks. Clay still does some jobs better — big storage jars and shipping amphorae — so they are here too (Pottery, The Potter's Wheel).

How it works

Glass is worked as it stiffens. At about 1,100 °C (bright yellow-orange) soda-lime glass is like thick honey; at 900–1,000 °C (orange) it is blown and shaped; by about 700 °C (dull red) it is too stiff to move. A piece cools from working heat in 20–60 seconds, so glassware is made in a rhythm of work, reheat, work, always turning so it does not sag.

Even walls survive; uneven walls crack. Thick and thin parts cool at different speeds and lock in strain, so a heavy base under a thin wall is the commonest place for a crack. Keep walls even, and anneal every piece: hold it at about 500–550 °C so the strain relaxes, then cool it slowly.

Three ways to shape. Free-blowing gives any shape, each a little different. Mould-blowing gives bottles of one size, fast. Pressing a lump into a mould with a plunger needs no blowing skill and makes thick open shapes: tumblers, bowls, plates, insulators.

Which glass. Soda-lime glass (Glass) suits everything here; green or brown wood-ash glass suits bottles and shades their contents from light. Lead crystal is brilliant, but lead leaches into wine and spirits stored in it: do not make it for food or drink.

What you need

Item Notes
Furnace, glory hole, annealing oven Glass; the annealer holds 500–550 °C for hours
Blowpipes and punties 1.2–1.5 m iron tubes (bore about 1 cm) and solid rods 12–15 mm thick
Marver A flat polished stone or iron slab
Jacks Spring tongs with two blunt blades, for necking and opening (Blacksmithing, Springs)
Shears For trimming hot glass (Scissors, Shears and Folding Knives)
Wooden blocks and paddles Pear, cherry or beech, kept soaking in water
Lipping tool, moulds Below
Sand and emery Grinding stoppers (Abrasives and Grinding Stones)
Two polarisers Checking strain (Polarised Light)

A glass workshop is a team: a gaffer who shapes, a servitor who gathers and blows, and a helper who carries pieces to the annealer.

Where to find it

The batch — sand, wood ash or soda, and limestone — is in Glass; save every chip of scrap as cullet. Cork is the thick, spongy bark of the cork oak, an evergreen oak of the western Mediterranean, stripped every nine years or so without killing the tree; elsewhere, turn stoppers from fine wood and boil them in beeswax. Pine resin lines clay jars (Finding and Preparing Clay).

Bottles

Two-piece bottle mould cut through, closed Blowpipeblow firmly, steadily Cast-iron halfwarmed to ~300 °C Seamhalves hinged Glasswalls 3–4 mm Raised baseforms the punt Vent1 mm handle 75 mm body Neck finishes String rimfor a tied cork Tooled lipfor a driven cork 18–19mm Crownfor a crimped cap 26 mm bead Lipping tool turn the bottle against it one or two turns Plugsets the bore Jawsshape the outside spring bottle neck
Fig. 1 Left: a two-piece hinged bottle mould, cut through. The gather is blown inside the closed mould and swells to fill it; the punt rod pushes up the base. Right: three neck finishes — a laid-on string rim for a tied cork, a tooled lip with an 18–19 mm bore for a driven cork, and a crown finish with a 26 mm bead for a crimped cap — and the lipping tool that forms them.

A wine bottle of 750 ml is about 75 mm across the body and 300 mm tall, with walls 3–4 mm thick and a base 5–8 mm thick, and weighs 500–900 g. Beer and soda bottles of 330–500 ml are shorter and thicker. Bottles for anything fizzy must be round, with thick, even walls and a domed base; square bottles burst (Beer, Wine and Cider).

Free-blown bottles

  1. Gather twice, to about the size of a large orange; marver it, blow a first bubble, reheat.
  2. Swing the pipe down like a pendulum while blowing gently: the bubble stretches into a long body.
  3. Rest the bubble on the marver, pipe upright above it, and press gently to flatten the bottom.
  4. Push up the base 1–3 cm with a pointed rod. This dome — the punt — strengthens the base, stops the bottle rocking, and gives the punty a grip.
  5. Stick the punty to the punt, crack the bottle off the pipe, and finish the neck.

Mould-blown bottles and the bottle mould

A bottle mould gives every bottle the same capacity — so a bottle can serve as a measure — and lets a less skilled blower work fast.

  • The dip mould. A one-piece open cylinder, slightly wider at the top so the bottle lifts out. It shapes the body; the blower shapes shoulder and neck by hand above it. Carve it from wet pear or cherry wood, or make it of fired fireclay or iron.
  • The two-piece hinged mould shapes the whole bottle. Cast the halves in grey The Blast Furnace and Cast Iron from a wooden pattern 1 % larger than the bottle (Metal Casting), hinge them, fit long handles, polish the inside, and drill a few 1 mm vents at base and shoulder to let air out.
  • Wooden moulds must be kept soaking wet — the steam cushion stops burning and sticking — and last a few hundred bottles. Iron moulds last years; warm them until a dry pine splinter pressed on them chars (about 300 °C). Too cold leaves wrinkles; too hot, the glass sticks.

Step by step:

  1. Gather the same amount each time (weigh finished bottles to learn it), and blow a small bubble, the parison, about half the bottle's size. Reheat it evenly.
  2. Lower it into the mould, the helper closes it, and blow firmly and steadily; in a smooth round mould, turn the pipe too, and the bottle has no seam.
  3. A raised mould bottom forms the punt. Open the mould, stick on the punty, crack the bottle off the pipe, and finish the neck.

Finishing the neck

The neck is opened and closed hundreds of times: it must be round, smooth and of the right bore. Reheat the cracked-off end to orange, then:

  • String rim — for a cork tied down with string or wire: wind a thread of hot glass once round the neck 5–10 mm below the mouth.
  • Tooled lip — for a driven cork: put the lipping tool's plug in the mouth, close its jaws round the outside, and turn the bottle a turn or two. Make the bore 18–19 mm, parallel for the first 4 cm, checked with a tapered wooden plug gauge.
  • Crown finish — add a ring of glass and tool it into a bead about 26 mm across with a flat top for a crimped cap (Tins, Cans, Drums and Tanks).
  • Swing-stopper finish — a thick lip with a strong collar for the wire.

Fire-polish the mouth and anneal.

Corks. Punch cylinders about 24 mm across and 45 mm long from cork bark with a sharpened brass tube and boil them 10–15 minutes. Squeezed into an 18.5 mm bore, a cork grips by its own spring. Seal with beeswax or pitch for long keeping; tie down corks on fizzy drinks.

Good bottle: stands without rocking; walls even (thin spots look paler against the light); no bubbles at the lip; the cork does not leak with the bottle on its side for a day. Bad bottle: a thick base under thin shoulders, an oval mouth, or a bubble ("seed") at the lip — that is where it will crack.

Drinking glasses

1 Blow the bowl 2 Pull the stemadd a small gather,draw out with the jacks 3 Open the footsecond gather, flattenedwith a wet paddle 4 Punty onthe foot; crack off,open and trim rim blowpipe jacks foot paddle punty Tumbler200–250 ml 70–75 mm 95–110mm base 4–6 mm Wine glass bowl 65–80 mm across stem 50–80 mm6–10 mm thick foot at least as wide as the bowl Bowl200–350 ml, walls 1.5–2 mm,rim fire-polished smooth
Fig. 2 A stemmed wine glass in four stages. 1: the bowl is blown on the pipe. 2: a small gather is added to the bottom and pulled into a stem with the jacks. 3: a second gather is opened into a flat foot with the jacks and a wet paddle. 4: the punty is stuck to the foot, the glass is cracked off the pipe, and the rim is trimmed, opened and fire-polished. Below: the finished wine glass and a plain tumbler with their usual sizes.

The tumbler

A plain straight-sided drinking glass of 200–250 ml: about 70–75 mm across and 95–110 mm tall, walls 1.5–2.5 mm, base 4–6 mm.

  1. Blow a bubble the size of the glass, flatten its bottom on the marver, and shape the sides straight in a wet block.
  2. Stick the punty to the centre of the base and crack the glass off the pipe.
  3. Reheat, shear away the ragged neck while turning, and open the rim with the jacks — one blade inside, one out — until the sides are straight. Fire-polish and anneal.

Crack-off, the faster way: blow tall bubbles in a mould and anneal them; scratch a ring round each with a hard point, touch the scratch with a hot iron ring, and it splits cleanly. Grind the rim flat with sand and water and fire-polish it.

The stemmed wine glass

A wine glass has three parts: a bowl, a stem and a foot. The stem keeps a warm hand off the wine; the foot must be wide enough not to tip.

Sizes: bowl 200–350 ml, about 65–80 mm across; stem 50–80 mm long, 6–10 mm thick; foot at least as wide as the bowl's rim, 65–80 mm, and 2–3 mm thick, flat or slightly domed.

  1. Bowl. Blow and block the bowl on the pipe.
  2. Stem. The servitor drops a small gather onto the centre of the bowl's bottom; the gaffer shears it and, rolling the pipe on the arms of the glassmaker's chair, draws it into a stem with the jacks.
  3. Foot. A second gather on the stem's end is opened into a disc with the jacks and flattened with a wet paddle.
  4. Transfer to a punty stuck to the foot; crack the bowl off the pipe; shear, open and fire-polish the rim.
  5. Anneal; grind the punty scar on the foot flat later.

Good glass: stands straight, stem centred, rim even. A rocking foot or leaning stem means the pipe was turned unevenly; a crack where stem meets bowl means the parts were at very different heats — reheat both before joining.

Carafes and decanters

A carafe is a plain glass jug of about 1 litre: a round body 110–130 mm across on a wide flat base, and a neck 35–45 mm wide flared into a lip with the jacks, with a small spout pinched in while it is soft. Blow it like a free-blown bottle.

A decanter is a carafe with a ground stopper. Give it a neck bore of 20–25 mm. Make the stopper from a small gather, tooled to a taper of about 1 in 10 with a finial to hold, and anneal it. Grind stopper and neck together with fine sand and water, then emery, until both are evenly frosted (30–60 minutes; Laboratory Glassware), and scratch the same number on both: a ground stopper fits only its own neck.

Good one: turned upside down with water inside, the stopper does not leak; the decanter does not tip when full.

Pressed glass

Hand glass press cut through, pressing a tumbler Clay vessels Lever1–1.5 m, one pull Plungershapes the inside Ringforms the rim Glasswalls 3–4 mm+ Mouldcast iron, kept hot guide No undercuts: sides slope outward 2–3° so the piece tips out Stoppercork or clay, pitch cap handles Toestands in sand, stacks Amphora~1.1 m, ~25 l Storage jar5–50 l Lid in a gallery
Fig. 3 Left: the hand glass press, cut through. A cast-iron mould sits under a plunger on a lever; a ring on top holds the glass in and forms the rim. A sheared lump of glass is dropped in, the lever is pulled once, and the plunger squeezes it into every corner. Right: a clay amphora — pointed toe, two handles and a narrow neck stopped with clay or cork and pitch — beside a wide-mouthed lidded storage jar.

Pressed glass needs no blowing. A crew of three at one press makes a tumbler, bowl, plate, salt cellar, jar lid or electrical insulator (Insulators, Cables and Electrical Fittings) every 20–40 seconds.

The press: an iron or timber frame on a heavy bench, with a lever of 1–1.5 m driving a plunger down through a guide into a cast-iron mould (the outside shape). A ring on top of the mould shapes the rim and stops glass squeezing out. Heavy pieces need a screw press (Presses, Punches and Dies).

Rules for the mould: no undercuts, and sides sloping outward at least 2–3°, so the plunger lifts out and the piece tips out; walls at least 3–4 mm thick; any pattern or capacity mark cut into the mould comes out raised on the glass. Keep mould and plunger at pine-splinter heat (about 300–450 °C).

Step by step:

  1. The gatherer lets a gather drip into the mould and the presser shears it off at the right weight.
  2. Pull the lever down in one smooth stroke; hold 2–5 seconds.
  3. Lift plunger and ring, tip the piece out onto ash or a warm plate, fire-polish the rim if dull, and anneal.

Good piece: smooth, bright surface, sharp pattern, full rim. Bad piece: wrinkled "chill marks" (mould too cold), a ragged, short rim (too little glass or too slow), a fin of glass at the ring (too much glass), sticking (mould too hot).

Storage jars and amphorae in clay

The storage jar

A household storage jar of 5–50 litres for grain, oil, pickles or water has a wide body, a mouth of 10–20 cm for a hand or ladle, and a lid. Throw small ones in one piece; throw big ones in two or three sections joined leather-hard (The Potter's Wheel), or coil them (Pottery) — coil-built jars as tall as a person stood in Bronze Age palace storerooms.

  • Walls 8–15 mm, thicker at the base, with a rolled rim that does not chip.
  • Seal the inside with a lead-free glaze (Glazes) or salt glaze, or use stoneware, which holds water unglazed (Stoneware and Porcelain). Line earthenware for oil or wine by swirling hot pine resin or beeswax round the warmed jar and pouring out the surplus.
  • Lids sit in a gallery (inner ledge); or tie on a cloth sealed with wax; or, for pickles, use a water seal moat (Preserving Food).

The amphora

An amphora is a tall clay shipping jar with two handles, a narrow neck and a pointed toe. The Romans shipped wine, oil and fish sauce in them across the whole Mediterranean. A typical wine amphora was about 1–1.2 m tall and held about 25 litres; globular oil amphorae held up to about 70.

  • Why the shape works: the narrow neck is easy to seal; the handles and the toe give three grips for lifting and pouring; the pointed toe stands in sand and lets jars nest in layers in a ship's hold, where flat bases would break.
  • Making: throw the body in two parts and join them, add the neck, pull and attach the handles leather-hard, add a solid toe, and fire hard. Line wine amphorae with pine pitch.
  • Sealing: a cork or clay plug capped with clay or pitch, often stamped with the maker's mark.

Use them where barrels cannot be made (Barrels and Cooperage) and for oil, which seeps through wood; pack them in straw for travel (Sacks, Boxes, Crates and Packaging).

Annealing so they do not crack

Every glass piece in this chapter goes into the annealer while still hot, never allowed to cool in the open air first.

Piece Hold at 500–550 °C Then cool to cold over
Wine glass, tumbler (walls 2 mm) 20–30 minutes 6–8 hours
Bottle (base 5–8 mm) 1 hour 12–24 hours
Pressed piece (walls 4–8 mm) 1 hour 12–24 hours
Thick decanter base, glass insulator (10–20 mm) 2 hours 24–48 hours

The lehr. A busy workshop uses a lehr: a long brick tunnel, hot at the furnace end and cool at the other, with trays pulled slowly through it over 4–12 hours, so it never has to be cooled and reheated.

Check the strain between two polarisers turned to make the view dark (Polarised Light). A well-annealed piece stays dark or faint grey; bright coloured bands round the base or punty mark mean strain — re-anneal or break it.

How to tell it worked

  • Thermal test. Plunge one piece from each batch from room-temperature water into water 40 °C warmer. A good piece survives.
  • Pressure test for bottles meant for fizzy drinks: fill one from each batch brim-full of water, with no air, and pump it to about 6 atmospheres — twice what bottled beer reaches — with a hand pump and gauge (Pumps, Pressure and Vacuum Gauges). Sparkling wine reaches 5–6 atmospheres in a cool bottle and 7–8 in a warm one, so test bottles meant for it to at least 12. Water stores little energy, so a weak bottle just cracks.
  • Ring test. Tapped with a fingernail, sound glass rings; a dull clunk means a hidden crack.
  • Capacity. Bottles from one mould agree within 1–2 % (Measurement from Scratch).
  • Clay jars hold water for a day without sweating.

Note Troubleshooting. Bottles crack across the base days later → base much thicker than walls, or poor annealing; blow more evenly and anneal longer. Bubbles ("seed") all through the glass → melt not fined long enough; hold the pot at top heat longer before working (Glass). Small white specks ("stones") → unmelted batch or crumbs of crucible; melt hotter and longer, and skim. Wavy lines ("cords") in the glass → poor mixing of the batch; grind and mix it better, stir the melt. Glass turns cloudy after months → too much alkali, not enough lime or sand (Glass); for food and drink, test a new batch by boiling a chip in water for an hour. Clay jar sweats or smells sour → porous body; fire hotter, glaze, or line with wax or resin.

Dangers

Danger Burns and flying glass. Hot glass looks exactly like cold glass once it stops glowing, and holds heat for minutes. Never touch a piece that has just been worked; never pick up glass from the floor near the furnace without tongs. When glass cracks off a pipe, or a strained piece shatters, it throws needle-sharp fragments: wear eye protection and keep children away from the bench.

  • Bursting bottles. A bottle of fermenting drink can explode with enough force to cut an artery (Beer, Wine and Cider). Use only round, thick bottles that passed the pressure test, store them boxed, and cover your face when checking them.
  • Furnace glare. Staring into the glory hole for years damages the eyes (glassblower's cataract). Wear dark glass goggles (Spectacles) when looking into the fire.
  • Lead. Do not make lead glass or lead glazes for drinking vessels or food jars (Lead).
  • Dust. Grinding glass and dry clay makes fine silica dust that scars the lungs: grind wet, sweep wet.
  • Chipped rims cut lips and leave slivers in drink. Grind off or throw away chipped glasses.

What this unlocks

Bottles make possible the trade in wine, vinegar, oil, medicines and chemicals (Making Medicines, Pharmacy: Tablets, Capsules, Ointments and Inhalers), and safe sealed storage (Canning and Bottling). The skills of the bottle mould and the press lead to glass insulators (Insulators, Cables and Electrical Fittings), lamp chimneys (Lamps and Candles), light bulb envelopes (The Light Bulb), lenses (Lenses) and the Laboratory Glassware of the chemist. Clay storage jars underpin Preserving Food and Granaries and Food Storage.

How it was first done

The first glass vessels were made in Mesopotamia and Egypt around 1500 BC by winding hot glass round a core of clay and dung, which was scraped out afterwards. Glassblowing was invented on the Syrian and Palestinian coast around 50 BC, and within a century Roman workshops were blowing cups, flasks and square storage bottles, some into moulds — the first mass-produced glassware. Medieval Europe made green "forest glass" from wood ash; Venice made clear cristallo from the 1400s; and George Ravenscroft in London made lead crystal in the 1670s.

Strong, dark, coal-fired English wine bottles appeared in the mid-1600s and made bottled wine and sparkling wine possible. Henry Ricketts of Bristol patented a three-part iron bottle mould in 1821 that shaped body, shoulder and neck at once. Glass pressing spread in the United States in the 1820s, and in 1903 Michael Owens built a fully automatic bottle machine that put hand bottle blowers out of work within twenty years. Clay storage jars are far older than glass; the Canaanite trading jar of the Bronze Age grew into the Greek and Roman amphora, which carried the trade of the Mediterranean for more than a thousand years until the wooden barrel replaced it in the north.