◆ Rebuild

Part 15 · Knowledge and Science

Ink

How to make permanent black ink from soot and gum, or from oak galls and iron; how to cut quill and reed pens; and how to make the thick, oily ink that a printing press needs.

Difficulty
●●●●●
Time
An afternoon for carbon ink; a week for iron-gall ink; 20 minutes to cut a pen; a day for printing ink
Steps from zero
2 prerequisites →

You need first

Charcoal

This unlocks

Pens, Nibs and Writing InstrumentsPrinting
The full path from nothing — 2 steps before this one
  1. Fire
  2. Charcoal
  3. Ink

Do them roughly in this order. See it on the tech tree →

Why it matters

Ink turns any flat surface — Paper, parchment, bark, cloth, wood — into a record. Scratching letters into wax or clay is slow; a good pen and good ink let a trained hand write a thousand words an hour. The black inks in this chapter are among the most durable things people have ever made: carbon ink written in Egypt more than 4,000 years ago is still black today.

Ink is also the second half of Printing: a printing press is useless without an ink that sticks to metal type and transfers cleanly to paper.

How it works

A good ink has three parts:

  • A colouring matter that is very dark and very fine. Either carbon — soot, which is nearly pure carbon in particles far smaller than a grain of flour — or a dark compound made inside the ink by a chemical reaction.
  • A binder that glues the colour to the page: a gum, a glue or an oil.
  • A carrier that lets it flow: water for pen ink, oil for printing ink.

Carbon ink is simply soot held in gum and water. Carbon never fades or rots, but it sits on the surface, so it can be washed off parchment while fresh.

Iron-gall ink works by chemistry. Oak galls are full of tannin — the same bitter, mouth-drying substance as in strong tea and oak bark. When tannin meets dissolved iron, the two join into a compound that turns black in air (the same reaction that blackens an iron knife cutting an apple or an oak branch). Because the ink soaks into the page before it darkens, it bites in and cannot be washed or scraped away easily.

What you need

Ink Ingredients Tools
Carbon ink Soot (lampblack), gum arabic or another water-soluble gum, clean water Oil lamp, a clay or stone plate, feather, smooth grinding stone and muller
Iron-gall ink Oak galls, green vitriol or iron dissolved in vinegar, gum arabic, rain water Pottery jar, cloth for straining
Printing ink Lampblack, linseed oil Iron or clay pot, fire, grinding stone
Pens Goose or other large flight feathers; dry reeds A very sharp small knife, a hard flat block

Where to find it

  • Soot comes from any smoky flame: oil lamps burning vegetable oil or animal fat, resin-rich pine wood and burning tar. Lamp soot is the finest; for soot on a larger scale see Lampblack and Carbon Black. Finely ground Charcoal also works, but it is greyer and grittier unless ground for hours.
  • Oak galls are hard, round balls 1–2.5 cm across on oak twigs and leaves, made by the plant around the grub of a tiny wasp. Fresh ones are green to brown and heavy; collect them in late summer, before the wasp has bored its exit hole — hole-free galls contain the most tannin. The best of all are the small, knobbly "Aleppo" galls of the Middle East, which are over half tannin. Other tannin sources work, more weakly: oak bark, sumac leaves, pomegranate rinds, chestnut and alder bark, and acorn cups.
  • Gum arabic is the dried sap of certain acacia trees of the dry African and Arabian bush. It oozes from wounds in the bark and hardens into clear to amber, glassy lumps that dissolve completely in water. Substitutes: the amber gum that oozes from cherry, plum, apricot and peach trees in summer (soak it a day; it dissolves more slowly), egg white beaten and left to settle, or thin hide glue.
  • Green vitriol (iron sulfate) forms as green or white crusts on rocks containing pyrite, especially in damp shale and old mine tunnels. It tastes sharply metallic and dissolves in water to a pale green liquid. See Sulfuric Acid, where it is made on purpose.
  • Feathers: the five or six large outer flight feathers of each wing of a goose, swan or turkey; crow feathers for very fine writing. Birds shed them naturally in summer — look along lake shores.
  • Reeds: hollow-stemmed reeds and canes from marshes and river banks, cut when dry and pale.
  • Linseed is flax seed. Press it for oil (see Oils and Pressing).

Method 1: Carbon ink

Clay tile, kept coolswap it when it gets hot soot builds upjust above the flame 3–5 cmflame tip just licks the tile Long wicksmoky flame Oil lampplant oil or animal fat Scrape with a featherevery 15–30 minutes jar oflampblack
Fig. 1 Collecting lampblack. A cool clay plate held just above the tip of a smoky flame catches fine soot. Scrape it off with a feather every quarter of an hour.

Make the lampblack

  1. Fill a shallow clay lamp with oil or melted fat and lay a thick wick of twisted plant fibre in it. Pull the wick out until the flame is tall and smoky.
  2. Hold a cool, smooth surface — the underside of a clay plate or pot, or a flat stone — 3–5 cm above the tip of the flame, so the flame just licks it. A black velvety layer builds up. If the plate gets too hot, the soot burns away; swap for a cool one.
  3. Every 15–30 minutes, scrape the soot into a jar with a feather. Expect only a few grams an hour per lamp; run several lamps at once.
  4. Cleaning the soot (recommended). Raw soot is often oily and refuses to mix with water. Pack it into a small clay pot, seal the lid with clay, and set it in hot embers for an hour. When cool, it is drier and mixes far better.

For larger amounts, burn resinous pine wood or pine tar slowly in a small enclosed chamber with a long flue; the soot settles inside, the finest farthest from the fire. This is how Chinese ink-makers worked.

Mix the ink

  1. Soak 1 part gum arabic in 2 parts warm water overnight until it is a clear syrup.
  2. Put 10 g of soot on a smooth stone slab and add gum syrup a few drops at a time, working it in with a flat-bottomed stone (a muller) or a knife blade, until it forms a stiff, smooth paste. Use about 10–15 g of gum (in its syrup) in all.
  3. Grind for 30–60 minutes. The longer you grind, the finer, blacker and smoother the ink.
  4. Thin it with clean water, a little at a time, until it flows easily from a pen but still makes a dense black line — about 50–100 mL in all.
  5. Store in a stoppered pot. A clove, or a few drops of strong vinegar or spirit, discourages mould.

Tip Ink sticks. Chinese and Japanese ink is stored dry: knead soot with warm, thick hide glue into a stiff dough, press it into a small block, and dry it slowly for weeks. To write, rub the stick with a few drops of water on a smooth stone. Dry ink keeps for decades and never spills.

Method 2: Iron-gall ink

  1. Crush 60 g of oak galls to a coarse powder between stones. Don't grind to dust; it makes straining harder.
  2. Extract the tannin. Put the galls in a jar with 500 mL of rain water (soft water — hard water dulls the ink). Either leave it in a warm place for 1–2 weeks, stirring daily (it may grow a skin of mould; skim it off), or simmer it for an hour. The long soak gives a blacker ink.
  3. Strain the brown liquid through a cloth.
  4. Add the iron. Dissolve 30 g of green vitriol in a little water and stir it in. The liquid turns dark grey-violet at once.
  5. Add the binder: about 25–30 g of gum arabic, dissolved. The gum thickens the ink so it flows well and holds the dark particles in suspension.
  6. Let it stand a day or two and pour the clear ink off the sediment. It writes pale grey or violet and darkens to deep black within hours as it meets the air.

Note No green vitriol? Use iron and vinegar. Put a large handful of clean iron scraps, filings or rust-free nails into 500 mL of strong vinegar. Leave it loosely covered for 1–2 weeks until the liquid is reddish-brown. This "iron liquor" (iron acetate) does the same job: add it to the gall extract a spoonful at a time, testing a stroke on paper after each addition, until the ink dries as black as it will go. See Iron (the Bloomery) for the metal itself.

Keep the iron in balance. Twice as much gall as vitriol, by weight, is a safe rule. Too much iron leaves a brown halo around the letters and, over centuries, the excess acid eats through the paper — many medieval manuscripts have holes where the ink was. Too little iron gives a weak grey.

Pens

Cutting a quill

1 · Scoopslanting cut on theunderside, 2–3 cm 2 · Slit6–10 mm upthe centre 3 · Shoulderstaper both sidesevenly to the tip 4 · Nibcut straight downon a hard block 5 · Finishedsquare tip 1–2 mm(shown enlarged) side viewfrom belowfrom belowside viewfrom below
Fig. 2 Cutting a quill. A long scoop on the underside, a short central slit, two even shoulders, then a clean square cut across the tip on a hard block.
  1. Prepare the feather. Strip off most of the vane (the feathery part) — you need only the hard shaft. Cut the quill to about 18–20 cm. Scrape the waxy outer skin off the hollow barrel with the back of a knife.
  2. Cure it (optional but better). Raw quill is soft and springy. Soak the barrel in water overnight, then push it into a pot of hot dry sand — about 170 °C, hot enough that a drop of water spits away instantly, but not so hot that dry grass laid on it chars within seconds. After 10–20 seconds the barrel turns from milky to clearer and harder. Pull it out, roll it round, and let it cool.
  3. The scoop. Hold the quill with its curve bending down. On the underside, cut a long slanting scoop 2–3 cm long, removing half the barrel's thickness. Clean out the dry membrane inside with a twig.
  4. The slit. Lay the quill back-up on a hard block. Set the knife edge across the middle of the tip and press down to split a slit 6–10 mm long up the centre. The slit lets the two halves of the nib flex and draws ink down by capillary action.
  5. The shoulders. Cut both sides of the scoop evenly so they taper towards the tip, with the slit exactly in the middle.
  6. The nib. Put the tip inside-down on the hard block and cut straight down across it. A square cut 1–2 mm wide gives an edged pen, which makes thick and thin strokes as you write; cut a little narrower for fine notes, wider (3–4 mm) for large letters. Left-handers cut the tip at a slight slant.
  7. Dip and write. Re-cut the nib when it softens and blurs — a goose quill gives a day or two of writing per cut, and can be re-cut many times.

Use a very sharp small knife — the original "penknife". A fresh flint or obsidian flake (see Stone Tools) works.

Cutting a reed pen

Choose a dry, straight, hollow reed about as thick as a pencil to a finger. Cut a section 20 cm long with a joint near the far end. Then cut it exactly like a quill: scoop, slit, shoulders, nib. Reeds are stiffer and hold less ink, and give a bolder line; they were the pen of the ancient world and are still used for Arabic calligraphy. A bundle of fine animal hair bound into the end of a reed makes a brush, the writing tool of China and Japan.

Method 3: Printing ink

Water-based ink beads up and runs off metal type. Printing needs a thick, sticky, oil-based ink.

  1. Make the varnish. Heat raw linseed oil in an iron or clay pot, outdoors, with a lid close by. Fill the pot no more than one third. Keep it just short of smoking hard (around 250–300 °C) for several hours, stirring, until it is as thick as honey. Test a drop on a cold stone: when cool, it should be sticky and pull out into a short string between finger and thumb.
  2. Grind the ink. On a stone slab, work 1 part lampblack into about 4–6 parts varnish, by weight, with a muller, until there are no grains at all.
  3. Judge it. It should be stiff, like soft butter or thick honey, and tacky. Lift a knife out of it: good ink breaks off short rather than pulling a long thread.

Early printers made their varnish by setting the hot oil alight on purpose and smothering it with a lid. It works but is very dangerous; slow heating is safer.

How to tell it worked

  • Blackness: a stroke should dry deep black, not brown or grey. Iron-gall ink may need overnight.
  • Flow: the pen should write 5–10 words per dip without blotting or running dry.
  • Fastness: when dry, rub a damp finger over a stroke. Iron-gall ink should barely smudge; carbon ink on paper only slightly.
  • Edges: on good sized Paper, lines are sharp. Spreading, fuzzy lines mean the paper is unsized or the ink too thin — add gum.

Note Troubleshooting. Soot floats on the water and won't mix → bake the soot (see above), and mix it into gum syrup, not plain water. Carbon ink smudges when dry → too little gum. Ink cracks and flakes off → too much gum; thin with water, or add a drop of honey. Pen sprays and splutters → nib halves uneven or slit too long; re-cut. Pen won't hold ink → scoop too short or nib too wide.

Dangers

Danger Hot oil fires. Linseed oil heated for varnish can burst into flame and cannot be put out with water — water makes burning oil explode outwards. Work outdoors, away from buildings, with the pot on a stable fire. Keep a tight lid ready: to put out an oil fire, slide the lid on and take the pot off the heat. Never carry a burning pot.

Warning Oily rags can catch fire by themselves. Cloths soaked with linseed oil heat up as the oil hardens in the air and can burst into flame hours later. Spread them flat to dry outdoors, or keep them under water.

  • Green vitriol is poisonous to swallow — a few grams can kill a small child. Store it, and iron-gall ink, out of reach and clearly marked.
  • Soot is fine enough to reach deep into the lungs. Work in moving air and don't blow it about.
  • Knives: always cut away from the hand holding the quill.

What this unlocks

With ink and a pen you can keep records on Paper (see Writing and Numbers); steel nibs, spill-proof inkwells and fountain pens follow in Pens, Nibs and Writing Instruments. Oil-based ink makes Printing possible. The same carbon blacks and oil varnishes make paints, and the tannin-and-iron reaction makes black dyes for cloth and leather (see Dyes and Mordants).

How it was first done

Egyptian scribes wrote with carbon ink — soot in gum — and reed brushes by around 2600 BC, using red ochre ink for headings. Chinese ink of soot and animal glue is just as old, and ink sticks were refined over the next two thousand years. The Roman writer Pliny the Elder, in the 1st century AD, described papyrus soaked in gall juice turning black when touched by vitriol; by the early Middle Ages iron-gall ink had become the main ink of Europe and the Islamic world, and stayed so until the 20th century — Leonardo da Vinci and Johann Sebastian Bach wrote with it. The Greeks and Romans wrote with cut reeds; the quill pen came into use around the 6th century AD and ruled for 1,300 years until steel nibs took over in the 1800s. Gutenberg, around 1450, adapted the linseed-oil varnishes of Flemish painters to make the first ink for metal type.

Source: content/entries/knowledge/ink.md