◆ Rebuild

Part 5 · Cloth and Clothing

Tents, Sleeping Bags and Camping Gear

How to make a portable home of cloth — tarpaulin shelters, ridge, bell and frame tents with their poles, pegs and guy lines, ground sheets, sleeping bags and bedrolls, mosquito nets — and the small kit that goes with them, the camp stove, mess tin and canteen.

Difficulty
●●●●●
Time
A tarp in a day; a ridge tent in 4–6 days of sewing; a bell tent in 1–2 weeks; a mosquito net in 2–3 days once the netting is woven
Steps from zero
9 prerequisites →

You need first

Ropewalks and SailclothSewing, Needles and Thread

This unlocks

—
The full path from nothing — 9 steps before this one
  1. Cordage and Rope
  2. Stone Tools
  3. Basic Woodworking
  4. Farming from Seed
  5. Spinning and Weaving Cloth
  6. Flax, Hemp and Linen
  7. The Loom
  8. Sewing, Needles and Thread
  9. Ropewalks and Sailcloth
  10. Tents, Sleeping Bags and Camping Gear

Do them roughly in this order. See it on the tech tree →

Why it matters

A hut stays where you built it; a tent goes with you — to the summer pasture, the mine in the hills, the survey line, the camp after a flood or an earthquake. A good tent keeps a family dry for years and goes up in half an hour; a mosquito net over a sleeper is one of the cheapest life-savers there is (Infectious Diseases).

Sail canvas, rope, grommets and tarpaulins are taught in Ropewalks and Sailcloth; the quilt and fur sleeping bag in Quilting, Down and Warm Clothing; branch shelters in Shelter; felt yurts in Felt. This chapter is about making and pitching tents properly, and the gear that goes with them.

How it works

  • Shedding rain. Close-woven canvas is showerproof because its fibres swell when wet and close the gaps. Rain must run off quickly, so roofs need a steep slope: at least 45°, better 50–60° for plain canvas. On a flat roof water soaks through.
  • Tension. A taut tent sheds wind and rain; a slack one flaps, wears its seams and collects puddles. All tension runs from the pole tops along the ridge and seams to the guy lines and pegs. Pull guy lines in line with the seam they hold.
  • Wet cloth shrinks. Canvas and natural-fibre rope shrink when wet. A tent pitched tight in dry weather pulls its pegs or tears in the night's rain. Slacken the guys when rain starts, and tighten them as it dries.
  • Two skins beat one. A fly sheet — a second roof held 5–10 cm above the tent — sheds most rain and sun; the gap stops drips and keeps the tent cooler.
  • Breath is water. A sleeper breathes out a cupful or more of water a night. Without ventilation at the top it condenses and rains back down. Every tent needs a vent near the peak and a gap at the bottom.
  • Cold comes from below. The ground draws heat out faster than the air. Insulation underneath matters more than blankets on top.

What you need

Item For Notes
Canvas 250–350 g/m² Tents, fly sheets Close-woven hemp, flax or cotton (Ropewalks and Sailcloth, Cotton)
Lighter cloth 150–200 g/m² Light tents, inner tents Very tight plain weave; waxed or oiled
Rope Guy lines, ridge lines 5–7 mm three-strand for guys; 10–12 mm for a ridge rope
Twine and sail needles, palm Seams, grommets As for sails
Poles Tents Ash, spruce, hazel or bamboo, 3–5 cm thick
Pegs Anchoring Ash or oak; later forged iron (Blacksmithing)
Boiled linseed oil, beeswax Waterproofing Oils and Pressing
Fine cotton or linen thread Mosquito netting Hard-spun, 0.2–0.3 mm (Cotton, The Spinning Wheel)
Tinplate, sheet iron Stove, mess tin, canteen Sheet Metal and Rolling, Tin and Pewter

The tarpaulin shelter

A tarpaulin ("tarp") is a flat sheet with ties all round. It is the lightest shelter and the first one to make.

  1. Cut and hem a sheet 3 × 3 m or 3 × 4 m (sew narrow cloths together with flat seams, Sewing, Needles and Thread). Fold every edge twice into a 3 cm hem.
  2. Tie-out points: sew a loop of tape or rope at every corner, at the middle of each side, and every 50–60 cm along the edges, each through a square reinforcing patch 8–10 cm across. Sew another loop at the centre of the sheet, on top, to lift it.
  3. Waterproof it: brush on thin coats of boiled linseed oil, drying each for several days in the air, until it no longer lets water through; or rub beeswax into it and warm it in the sun. Oiled cloth is fully waterproof, but heavy and stiff.
  4. Pitch it. Tie a ridge rope 1–1.2 m high between two trees; throw the tarp over it and peg the sides out to make an A; or peg one long edge to the ground on the windward side and raise the other on two poles to make a lean-to facing a fire; or peg three corners down and raise the fourth on a pole for a "diamond" in high wind.

The ridge tent

RIDGE TENT FROM THE END pole spike through ridge grommet fly sheet 5–10 cm gap above roof roof 1.25 m ridge to eaves;1.4 m high at the ridge pole 4 cm ash 53° sod cloth ground sheet inside walls runner peg wall 0.4 m floor 1.5 m DRIVING A PEG ← tent this way rope in notch head leans away from the tent, about 45°; the pull drives it deeper
Fig. 1 A ridge tent pitched. Two upright poles hold a ridge; the roof slopes at about 50°. Short walls end in a sod cloth that turns in under the ground sheet. Guy lines run out in line with the seams to pegs driven leaning away from the tent. A fly sheet lies above the roof with a gap between.

The ridge tent — an A-shaped tent with a pole at each end — is the easiest real tent to sew and pitch. A size for two people and their kit:

Part Size
Floor 2.1 m long × 1.5 m wide
Height at the ridge 1.4 m
Walls 0.4 m high
Roof slope 1.25 m from ridge to eaves (about 53°)

Sewing it

  1. Roof and walls are one piece on each side: 2.1 m long × 1.65 m (1.25 roof + 0.4 wall), plus 3 cm hems. Run the cloths and their seams from ridge to ground, down the slope, so water runs along the seams, not into them. Use flat-felled or overlapped double-stitched seams.
  2. Ridge: sew the two sides together along the top and cover the seam with a ridge strip 8–10 cm wide, sewn down both edges. Put a reinforcing patch of 3–4 layers at each end of the ridge, with a grommet for the pole spike.
  3. Ends: each end is a five-sided piece — 1.5 m wide at the bottom, walls 0.4 m, peaked at 1.4 m. Split the front end down the middle for a door, overlapping 15 cm, closed with ties or toggles every 20 cm. At the back peak, sew a small vent under a hood of cloth.
  4. Eaves: at each point where wall meets roof, every 60–70 cm, sew a guy loop through a patch. Sew wall loops every 50 cm along the bottom edge for pegs.
  5. Sod cloth: a strip 20–25 cm wide sewn all round the bottom of the walls that lies flat on the ground inward, under the ground sheet. It stops draughts, insects and water creeping in.
  6. Fly sheet: a second roof the same shape, 30 cm longer at each end and reaching to 20 cm above the ground, with its own guys. It is held up on the same pole spikes, above the tent, by a spacer of wood or a ring 5–10 cm thick.

The canvas for this tent is about 11 m²; at 300 g/m², about 3.3 kg — plus the fly, poles and pegs.

Poles: two uprights of 4 cm ash or spruce, each with an iron spike 5–8 cm long at the top that passes through the ridge grommet. For carrying, cut each pole in two and join the halves with a ferrule, a 10–12 cm sleeve of sheet metal or metal tube (Metal Pipes and Tubes) fixed to one half. A ridge pole between the uprights makes the roof stiffer but is heavier.

Pitching: peg the four corners square, raise both poles together, peg the end guys, then the side guys and wall pegs. Adjust until the ridge is straight and the roof unwrinkled.

The bell tent

BELL TENT, 4 m ACROSS crown and cap 4–5 layers, vent hood centre pole 3 m gore seams wall 0.6 m door slit 1.2 m high guy at every seam Sleepers lie like spokes, feet to the pole. FROM ABOVE: 12 GORES ONE GORE (CUT 12) 1.05 m 3.1 m dashed: seam allowance
Fig. 2 A bell tent and its pattern. A single centre pole holds up a cone of canvas gores above a short wall. Guy lines run from every gore seam. The pattern: twelve tapered gores whose bottom edges together make the circumference.

The bell tent is a cone of canvas on one central pole, with a short wall all round. It stands up well to wind from any direction, sleeps 6–10 people lying like spokes with their feet towards the pole, and was the standard army tent for nearly a century.

  1. Size: diameter 4–5 m, pole 3 m, wall 0.6 m.
  2. Gores: the cone is sewn from tapered panels called gores. For a 4 m tent the circumference is π × 4 = 12.6 m. With 12 gores, each is 1.05 m wide at the bottom (plus seam allowance) and tapers to a point. Its length is the slant height of the cone: the cone rises 3.0 − 0.6 = 2.4 m over a radius of 2 m, so the slant is √(2.4² + 2²) ≈ 3.1 m.
  3. Sew the gores edge to edge with flat-felled seams. At the top, the points meet in a reinforced crown of 4–5 layers with a metal cap or a stout grommet for the pole spike, and a small canvas hood over a vent.
  4. Wall: a strip 12.6 m long and 0.6 m high (plus hems), sewn to the bottom of the cone, with a door slit 1.2 m high between two gores, and a sod cloth.
  5. Guys: one at the foot of every gore seam, 12 in all, each a 5–6 mm rope 3 m long with a runner, pegged 1.5–2 m out from the wall. Wall pegs every 50 cm.
  6. Pitching: peg the door and the opposite side, push up the pole from inside, then peg the guys round, each tightened a little at a time like tuning a drum.

Frame and wall tents

A wall tent (frame tent) has upright walls 1.2–1.5 m high and a ridge roof, supported by a frame of poles — two end frames of three poles each (an upright on each side and the ridge in between) or a pole at each corner. It is a room you can stand in and work in, and the tent for long camps, field hospitals and survey parties (Surveying and Levelling). A 3 × 4 m wall tent can take a small iron stove.

  • Frame: 5 cm ash or bamboo poles, joined at the corners with sheet-iron or forged sockets, or lashed.
  • Stove jack: where a stovepipe passes through the roof, cut a hole 5 cm larger than the pipe all round and sew in a sheet-metal plate with a collar, or a ring of several layers of tightly woven wool cloth well away from the pipe. Fit a spark-catching wire mesh cap on top of the pipe (Chimneys, Stoves and Heating).

Pegs, poles and guy lines

  • Wooden pegs: split ash or oak, 25–30 cm long, 3–4 cm square, pointed at one end. Cut a notch 3–4 cm below the head, on the side facing away from the tent, for the rope. Char the point lightly in a fire to harden it.
  • Iron pegs: 6–8 mm rod, 20–25 cm long, the top bent into a hook. They go into stony ground where wood splits.
  • Sand and snow: pegs pull out. Use long, wide pegs (45 cm × 5 cm), or tie the guy round the middle of a stick, a bag of sand or a stone and bury it crosswise 20–30 cm deep (a deadman).
  • Driving: angle each peg about 45°, its head leaning away from the tent, so the pull of the rope drives it deeper. Use a wooden mallet; a stone will split the head.
  • Guy lines: 5–7 mm rope, 2–3 m long. End guys from the ridge run out at about 45°; side guys from the eaves are pegged 1–1.5 m out from the wall. Fit each with a runner — a flat piece of hardwood, bone or horn 8–10 cm long with two or three holes, through which the rope passes so that it slides to tension and grips under load. Without runners, use a taut-line hitch.

Ground sheet

A ground sheet keeps damp out of the bedding. Make it from oiled canvas, waxed canvas or later rubberised cloth (Rubber, Raincoats, Oilskins, Umbrellas and Rubber Boots).

  • Make it slightly smaller than the floor inside the walls, so the sod cloth lies under its edge. A ground sheet that sticks out beyond the walls catches rain running off them and funnels it into the tent.
  • A better version is sewn into the tent with its edge turned up 10–15 cm all round (a "tub" floor), so no water can enter at ground level.

Sleeping bags and bedrolls

SEWN THROUGH: CHEAP BUT COLD shell cold lines at every seam filling squeezed to nothing BOX BAFFLES: WARM baffle wallslight cloth, 5–8 cm high lining full thickness Baffles run across the bag every 15–20 cm; each tube is filled with its share of down, then sewn shut. MUMMY BAG hood drawstring draught tube along the opening shoulders 160 cm round feet 100 cm round length: sleeper + 25–30 cm
Fig. 3 Sleeping bag construction. Sewing straight through both layers makes cold lines where the filling is squeezed to nothing. Box walls (baffles) keep the filling full thickness everywhere. A mummy bag is tapered to the body, with a hood, and closes with a draught tube along the opening.

The simple sleeping bag sewn from two quilts, the fur bag, and the rules of keeping warm at night are in Quilting, Down and Warm Clothing. Here are the improved bag and the bedroll.

The baffled down bag

  1. Shape: a mummy bag is cut to the body — about 160 cm round at the shoulders, 140 cm at the hips and 100 cm at the feet, and as long as the sleeper plus 25–30 cm — with a hood. It weighs less and warms faster than a rectangular bag (80 × 200 cm), but is harder to turn in.
  2. Shell and lining: tight-woven cotton or silk (Silk), close enough that down does not work through — at least 40 threads per cm, or waxed.
  3. Baffles: instead of stitching the outer shell straight to the lining, sew strips of light cloth 5–8 cm high between them, across the bag every 15–20 cm, making box-shaped tubes. Fill each tube with its share of washed down or feathers (Quilting, Down and Warm Clothing) through an open end, then sew it shut. A bag for frost (around −5 °C) needs 700–900 g of good down; feathers alone need about twice as much.
  4. Opening: down one side, closed with ties or buttons (Buttons, Buckles, Hooks and Zips), with a draught tube — a filled tube of cloth 5–6 cm across — sewn along the inside of the opening so no cold line forms.
  5. Hood with a drawstring, and a soft filled collar round the shoulders.

The bedroll: a canvas sheet about 2 × 2.2 m, oiled or waxed on the outside, folded around blankets or a quilt, with the sleeper lying on a pad of felt or a straw tick (Mattresses and Upholstery). In the morning everything rolls up together around the spare clothes and is strapped with two leather straps (Bags, Backpacks, Wallets and Luggage). It is heavier than a sleeping bag but needs no special sewing, doubles as a ground sheet, and can be carried on a horse or a cart for years.

The mosquito net

The net protects whoever sleeps under it from malaria and other diseases carried by mosquitoes (Infectious Diseases). It must have holes no larger than about 1.5 mm — smaller than a mosquito's body with its legs folded — and be tucked in all round.

Making the netting. Knotted netting (Knitting, Crochet and Netting) is far too coarse. Mosquito net is woven from fine cotton or linen yarn, 0.2–0.3 mm thick, in an open weave of about 6–8 threads per cm each way. An open plain weave lets the threads slide and the holes grow; leno (gauze) weave stops this. In leno, pairs of warp threads are twisted round each other between every weft pick, locking each weft in place, so the holes stay square. On a simple loom, twist each pair by hand with a pick-up stick before every pick; on a floor The Loom, half-heddles called doups do the twisting.

Making the net.

  1. Size: a box net for one sleeper is about 190 cm long, 100 cm wide and 150 cm high; for a double bed, 190 × 180 × 150 cm. Add 30 cm all round the bottom to tuck under the mattress or mat.
  2. Sew four walls and a top. Bind the top edges with a strip of strong cloth, with a loop at each corner to hang it from the roof, the tent ridge or four sticks.
  3. A round (bell) net — a cone of netting gathered at the top into a ring hung from one cord — needs one fixing point and suits tents and huts.
  4. Tuck it under the mattress all round before dark, and check inside with a lamp for mosquitoes before sleeping.

Treating it. A net dipped in insecticide kills or drives off mosquitoes that land on it, and protects even through small holes. Dried pyrethrum flower heads ground to powder and soaked in alcohol or oil give an extract that can be used to dip nets (Pests and Plant Diseases). Natural pyrethrum breaks down within days in sunlight, so re-treat often and keep the net out of the sun by day. An untreated but whole, well-tucked net still protects well.

The camp stove

  • Three stones and a small fire are the oldest camp stove (Cooking Without Pots).
  • Tin-can stove ("hobo stove"): a tin can 10–15 cm across (Tins, Cans, Drums and Tanks) with a row of holes 1 cm across round the bottom for air, a door cut in the side for feeding twigs, and a row of holes round the top for smoke. A pot sits on top. It boils a litre of water on two handfuls of twigs.
  • Folding plate stove: four plates of sheet iron 20 × 20 cm, hinged at the corners with wire pins, folding flat for carrying, with a grate of iron rods across. Wood or charcoal (Charcoal).
  • Alcohol burner: a tin or brass cup 6–7 cm across holding 30–60 ml of strong alcohol (Distillation), with a pot stand 3–4 cm above it and a windshield of sheet metal round both. 30 ml burns for about 10 minutes and boils about half a litre.
  • Pressure stove: paraffin (Petroleum and Refining) pumped under pressure through a tube heated by its own flame, so it turns to vapour and burns from a fine brass jet (Metal Pipes and Tubes). Hot and economical, but needs precise brasswork.

Mess tin and canteen

Mess tin: two nesting pans of tinplate or aluminium (Aluminium), about 17 × 13 × 6 cm and 15 × 11 × 5 cm, with folding wire handles. One is a pot, the other a lid, plate or frying pan. Fold them from sheet with soldered or folded corners (Sheet Metal and Rolling); never solder with lead where food touches — use pure tin, or fold and rivet the corners. Never heat an empty tinned pan: the tin melts at 232 °C.

Canteen: a water bottle for the belt or strap, holding 0.75–1 litre.

How to tell it worked

  • Tents: in rain, no drips inside except where something touches the cloth; the roof stays taut and wrinkle-free; no pegs pull in a night of wind.
  • Sleeping bag: you sleep through a cold night without waking from cold; held up to a lamp, the filling looks even with no thin lines.
  • Mosquito net: a mosquito placed inside a net bag cannot find its way out; no bites by morning.
  • Canteen and mess tin: filled, they do not leak when shaken upside down for a minute.

Note Troubleshooting

  • Drips through the roof → something touched the wet cloth, or the slope is too flat. Rub beeswax over the spot when dry; steepen the pitch; add a fly.
  • Sagging, flapping roof → guys not in line with the seams, or slackened in the dry. Re-tension in line.
  • Pegs pull out → drive them at 45° leaning away, use longer pegs, or bury deadmen.
  • Everything wet inside but no leaks → condensation. Open the vents and the door a crack.

Dangers

Danger Never burn charcoal, a stove or a brazier in a closed tent. Burning fuel without enough air makes carbon monoxide, a gas with no smell that puts sleepers to sleep forever. A stove inside a tent needs a proper chimney and a vent, and must be out before you sleep.

Danger Canvas burns fast. Keep candles and lamps well away from the walls and hang them from the ridge; keep stoves and fires at least 3 m from the tent on the windward side. Have a knife ready to cut your way out the back. Never refill a hot alcohol stove: in daylight its flame is almost invisible.

  • Where you pitch: never under dead trees or dead branches ("widowmakers"); never in a dry stream bed or narrow valley floor, where a storm upstream can send a flood in the night; not on the highest point in a thunderstorm.
  • Oily rags: cloths used for linseed oil can heat up and catch fire by themselves as they dry. Spread them flat outdoors or burn them.
  • Insecticide: pyrethrum is very poisonous to fish. Do not dip or wash nets in streams or ponds.

What this unlocks

Tents let people work far from home: on Surveying and Levelling lines, at Mining and Tunnelling camps, on Pack Animals journeys, in field hospitals (Nursing the Sick). The same cloth and seams lead to Kites and Parachutes and Balloons envelopes.

How it was first done

People have lived in tents for tens of thousands of years: skins over poles, like the tipi of the North American plains; the black tents of the Bedouin, woven from goat hair, which swells shut in rain; and the felt yurt of Central Asia (Felt). The Roman army carried leather tents of sewn goat or calf skin, one for each group of eight soldiers; pieces have been found at Vindolanda by Hadrian's Wall. In the 5th century BC the Greek historian Herodotus described Egyptian fishermen sleeping under their fishing nets to keep off gnats. In 1856 the American officer Henry Sibley patented a conical tent with one central pole based on the tipi, and conical "bell tents" served the British and other armies from the mid-1800s to the First World War. In 1876 the Welsh merchant Pryce Pryce-Jones sold the "Euklisia rug", a wool blanket that folded into a bag with a pillow pocket — an early sleeping bag, bought in large numbers by the Russian army. In 1892 Frans Lindqvist of Stockholm made the first Primus paraffin pressure stove, which Roald Amundsen took to the South Pole in 1911.

Source: content/entries/textiles/tents-and-camping-gear.md