◆ Rebuild

Part 2 · Earth and Fire

Scientific Glassblowing and Glass-to-Metal Seals

The glassblower's bench torch and the joins that make apparatus — butt seals, T-seals, bulbs, coils and ring seals in soft glass and borosilicate — and the hardest trick of all, sealing metal through glass so that it stays airtight for years. These are the envelopes of every lamp, radio tube, X-ray tube and neon sign.

Difficulty
●●●●●
Time
A week to build a bench torch; a month of daily practice for clean joins; a season to make reliable metal seals and tube envelopes
Steps from zero
19 prerequisites →

You need first

Laboratory GlasswareGlassThe Vacuum Pump

This unlocks

Fused Quartz and Halogen Lamps
The full path from nothing — 19 steps before this one
  1. Fire
  2. Stone Tools
  3. Cordage and Rope
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Basic Woodworking
  7. Hunting and Trapping
  8. The Kiln
  9. Pottery
  10. Hides and Leather
  11. Lime
  12. Mercury
  13. Lye and Potash
  14. The Wheel and Axle
  15. Glass
  16. The Lathe
  17. Laboratory Glassware
  18. Pumps
  19. The Vacuum Pump
  20. Scientific Glassblowing and Glass-to-Metal Seals

Do them roughly in this order. See it on the tech tree →

Why it matters

Laboratory Glassware showed how to draw tubing and bend, seal and blow it in a spirit-lamp flame. That makes test tubes and simple stills. The apparatus of later chapters needs more: a condenser whose jacket is fused to its inner tube, a mercury pump with a dozen joints that hold a vacuum (The Vacuum Pump), a bulb with wires through the glass (The Light Bulb), a radio valve with seven leads (The Vacuum Tube), a neon sign bent into letters (Arc Lamps, Neon and Fluorescent Lights), an X-ray tube (X-Rays).

These need three skills beyond the basics: a hot, steady flame (the bench torch); joins — tubes fused end to end, side arms, a tube through the wall of another, bulbs and coils — with even walls and no hidden strain; and glass-to-metal seals that stay gas-tight through thousands of heatings. A settlement that wants electronics must train several scientific glassblowers.

How it works

Expansion is everything

Everything grows when heated. Glass and metal joined hot shrink by different amounts as they cool; if the difference is large the glass cracks, at once or a week later. The figures are stretch per million per degree:

Material Expansion Seals to
Fused quartz 0.55 Molybdenum foil only
Laboratory borosilicate ("Pyrex") 3.3 Nothing well — use a graded seal
Tungsten-sealing borosilicate 3.6–4.0 Tungsten
Tungsten 4.5 Tungsten-sealing borosilicate
Molybdenum 5.0–5.5 Harder borosilicates
Iron–nickel–cobalt ("Kovar") about 5 Its own sealing glass
Iron with 46 % nickel ("platinite") about 9 Soft glass
Platinum 9.0 Soft soda-lime and lead glass
Soft soda-lime or lead glass 9–9.5 Platinum, platinite, dumet
Copper 17 Only as a knife-thin edge

Two glasses must not be mixed either: soft glass fused to borosilicate cracks every time. Keep each glass in its own labelled rack.

Wetting

Glass sticks not to bright metal but to the metal's oxide, which dissolves into the glass. Too little oxide and the glass sits on the metal like water on wax, and leaks; too much and the thick oxide is itself the leak. So every seal has a tell-tale colour (see How to tell it worked).

Annealing

A join cooled unevenly is left strained. Annealing — holding the piece where glass just relaxes, then cooling slowly — removes it: lead glass at 430–450 °C, soda-lime at 510–540 °C, laboratory borosilicate at 560 °C. Below the strain point (about 400, 470 and 510 °C) strain is locked in. Strain glows in colours between crossed polarisers (Polarised Light) — the glassblower's best inspection tool.

What you need

Item Details
Fuel gas Coal gas (Lanterns, Gas Lamps and Lighters), Natural Gas and Helium, hydrogen (Hydrogen, Oxygen and Gases) or propane (Petroleum and Refining)
Air blast Foot bellows with a weighted leather reservoir (Bellows) or a rotary blower (Bellows to Air Compressors)
Oxygen For borosilicate: Liquid Air, Nitrogen and the Noble Gases or electrolysis
Glass Soft-glass and borosilicate tubing and rod, sorted by size (Laboratory Glassware)
Tools Carbon (graphite) paddle, pick and reamer; tweezers; brass pinch jaws; carbon mandrels; a scoring file or diamond (Industrial Diamond and Hard Abrasives)
Blow hose 60–80 cm of soft rubber tube (Rubber) with a mouthpiece and swivel; corks
Annealing oven Firebrick box to 600 °C with a pyrometer (Electric Kilns and Furnaces, The Thermometer)
Polariscope and eye protection See Polarised Light and Dangers
Seal metals Platinum, nickel–iron, tungsten, molybdenum wire; copper tube

Where to find it

Glass ingredients and borax: Glass, Borax and Boric Acid. Platinum: grains in a few gold gravels (Platinum and the Platinum Metals, Gold and Silver) — rare, so most settlements need substitutes. Nickel for platinite and dumet: green garnierite and sulfide ores (Nickel and Cobalt). Tungsten: heavy dark wolframite in quartz veins near granite (Tungsten and Filament Wire); molybdenum: soft, greasy, lead-grey molybdenite flakes in similar veins (Molybdenum). Copper tube: Metal Pipes and Tubes.

The lamp-working torch

15–20 cm brass body, 15–18 mm bore Gas fills the body flows round the jet Blue inner cone gas and air mix here Work just past the cone tip Air or oxygen jet 5–6 mm bore (oxygen: 7–19 jets) 5–10 mm Spider centres the jet Outer flame more air = smaller, hotter Gas in via tap and flashback bottle Air in bellows and reservoir tap
Fig. 1 A gas–air bench torch in section. Gas fills the outer body; air (or oxygen) comes up a central jet and mixes with the gas only at the mouth, so the flame cannot flash back. Two taps set the size and the heat of the flame.

The gas–air bench torch

A surface-mix burner: gas and air meet only at the mouth, so the flame cannot run back inside.

  1. Body: brass or copper tube 15–18 mm bore, 15–20 cm long (Metal Pipes and Tubes), back end capped, gas inlet soldered on the side.
  2. Air jet: a 5–6 mm tube up the centre through the cap, ending 5–10 mm short of the mouth, centred by a three-legged wire spider.
  3. Taps: a ground-brass cone tap on each line, close to your hand (The Vacuum Pump shows how to grind one).
  4. Stand: a heavy iron base holding the torch pointing away from you at about 30°.
  5. Air: bellows into a reservoir (a leather bag under a weighted board) for a steady blast of about 20–50 cm water-gauge.

Light the gas alone — a lazy yellow flame — then add air. It shrinks, turns blue and roars, with a sharp inner cone; the hottest spot is just beyond its tip. More air gives a small, hot oxidising flame; less air a bushy reducing flame with a yellow tip, for warming and soot-annealing. Gas–air works soft glass of any size and borosilicate up to about 10 mm.

Oxygen, ribbon and hand torches

  • Gas–oxygen: replace the air jet with 7–19 fine jets of 0.8–1.0 mm bore fed with oxygen. At about 2,700 °C it works borosilicate tubing 50 mm across and, with hydrogen, softens quartz. Fit a non-return valve and a water bubbler flashback arrestor (gas bubbling through 10 cm of water in a closed bottle) on both lines.
  • Ribbon burner: a row of 30–60 small flames along a 15–40 cm manifold, for long even bends and coils.
  • Hand torch: a short surface-mix torch on a hose, for work too big to turn in the bench flame.

The basic joins

Rotation is everything: glass heated on one side sags. Hold the work palms up, like a flute, and roll it about one turn a second with both hands together. Cork the far end and fix the blow hose to the near end with a swivel, so you can blow without letting go.

The butt seal

  1. Warm both ends in the bushy flame, then heat them in the hot flame, turning, until the rims glow orange and just round.
  2. Touch them together squarely, all round at once.
  3. Heat a narrow band over the join, turning both pieces together. It thickens; blow gently back to full width, then pull a little to thin any ring.
  4. Repeat heat–blow–pull until there is no ring, ridge or line.
  5. Flame-anneal in the bushy flame, coat soft glass with soot from a yellow flame, and cool in the oven or a warm place.

For tubes of different widths, first draw the wider one down to a short cone matching the narrow one.

T-seals, bulbs and coils

  • T-seal: heat a spot on the tube with a sharp flame, blow out a bump, heat its top and blow it into a thin bubble; knock that off and melt the edge into a hole with a raised rim the width of the side arm. Butt seal the arm on, tilting and turning so every part of the circle passes through the flame.
  • Bulb: heat a band and push the ends together to thicken it; repeat until you have gathered a thick band about one and a half times as long as the bulb will be wide. Heat it evenly, take it out and blow while turning, keeping the ends in line.
  • Coil for a coil condenser (condenses vapour in a third of the length of a straight Liebig condenser): wrap a 2–3 cm carbon rod, or an iron rod in a layer of paper that will char. Fix the tube's end to it, heat a band with the ribbon burner and wind 6–8 mm tubing onto it at a steady pitch of about 1.2 tube widths, turns not touching. Cool, slide off, anneal, and seal the ends through a jacket with ring seals.

The ring seal

A ring seal joins an inner tube to the end of an outer tube around it — in every condenser jacket, gas-wash bottle, pump trap and vacuum flask (Cryogenics and Superconductors). It cracks more often than any other join, because the two tubes cool at different speeds.

  1. Centre the inner tube with a ring of glass-fibre cloth (Glass Fibre and Glass Wool) a little back from the joint.
  2. Heat the outer tube's end and draw it into a short shoulder until its rim just touches the inner tube all round.
  3. Fuse the rim on with a small sharp flame, turning both together; blow gently through the inner tube to smooth it.
  4. The seal must be as thin as the tube walls, curving smoothly from one tube into the other. A thick bead cracks.
  5. Anneal at once. Never let a ring seal cool in still air.

Glass-to-metal seals

nickel inside press ≥ 5 mm copper amber oxide layer bead of sealing glass hard-glasswall knife edge copper tube glass taper 10–20 mm 3.3 4.5 5.6 6.7 7.9 9 borosilicate soft glass each step 1–2 cm Matched wire platinum, dumet or platinite in soft glass Tungsten bead in tungsten-sealing borosilicate Housekeeper seal copper thinned to 0.02–0.05 mm yields Graded seal expansion of each glass Thread test two rods fused side by side, drawn into one thread straight: matched gentle curve: usable tight curl: add a step
Fig. 2 Four kinds of glass-to-metal seal. Left: a matched wire in a pinch. Centre left: a tungsten rod with a bead of sealing glass. Centre right: a copper tube thinned to a knife edge so that it yields as the glass shrinks. Right: a graded seal of several glasses in steps; below, the thread test that tells whether two glasses match.

Matched wires

  • Platinum in soft glass: clean the wire red-hot, melt a bead of glass onto it or squeeze it in a soft tube end, and bury at least 5 mm in glass. Keep wire thin, 0.2–0.5 mm, and save platinum by welding copper on outside and nickel inside (The Light Bulb).
  • Platinite (iron with about 46 % nickel) expands like soft glass and was the old French substitute. Melt it in a covered crucible (Alloy and Stainless Steels), draw it to wire (Iron and Brass Wire), coat it lightly with borax, and seal like platinum.
  • Dumet, the wire of ordinary lamps: a core of iron with about 42 % nickel sheathed in copper making up a fifth to a quarter of its weight, drawn to 0.3–0.6 mm. Pack the alloy rod tightly in a copper tube and draw them down together until they weld; dip the finished wire in hot borax solution and dry. The borax keeps the copper from over-oxidising and helps the glass wet it.

Tungsten in borosilicate

  1. Clean tungsten rod (0.5–1.5 mm): heat to dull red and rub it on a stick of sodium nitrite, or grind it bright on fine emery.
  2. Oxidise lightly in the oxidising flame to a straw-to-blue tint — not grey.
  3. Bead it with tungsten-sealing glass, turning, until the glass flows on. The interface should look golden-amber to coppery brown.
  4. Seal the bead into the work. Into laboratory borosilicate, put two or three graded steps between (old lamp makers used a bead of uranium glass).

The Housekeeper seal (copper)

Copper expands far too much for any glass, but thinned to a knife edge it stretches instead of cracking the glass. Turn or file the end of a copper tube to a 10–20 mm taper ending in an edge 0.02–0.05 mm thick — thin enough to flex under a fingernail. Anneal it, dip in borax solution, heat the edge dull red, and melt glass onto it, overlapping by 5–10 mm. A good seal is clear red. This joins big copper parts — such as the water-cooled anode of a transmitting valve — to glass.

Quartz expands almost not at all; only molybdenum foil 0.02–0.03 mm thick with knife edges, pinched in an oxy-hydrogen flame, seals into it. That is how quartz mercury lamps get current through: a target for a mature workshop (Fused Quartz and Halogen Lamps).

Graded seals

To join glasses that do not match, build a short tube of several glasses in steps.

  1. Make step glasses: melt soft and borosilicate cullet mixed 6:1, 5:2, 4:3, 3:4, 2:5 and 1:6 in small crucibles (Glass); draw each into rod and tube; label them.
  2. The thread test: fuse a rod of one glass side by side with a rod of the next and draw them into one thread about 0.3 mm thick. Cooling, it curls towards the glass that expands more. Straight means matched; a gentle curve is usable; a tight curl means put another step between. It needs no instruments.
  3. Build the seal by butt-sealing short pieces in order, each at least as long as the tube is wide (1–2 cm).
  4. Anneal at the temperature of the softest glass, and cool very slowly.

Soft glass to borosilicate takes four to six steps; quartz to borosilicate about seven.

Envelopes for lamps, tubes and signs

flare exhaust tube lead-in wires press hole blown through neck melted onto flare filament to pump sealed tip 1 Parts flare, exhaust tube, leads 2 Press the stem blow a hole to the tube 3 Seal in and pump 4 Tip off melt the tube shut
Fig. 3 Building a lamp or tube envelope. A flare tube, an exhaust tube and the lead-in wires are pressed together into a stem, with a hole blown through to the exhaust tube. The electrodes are mounted on the stem, the stem is sealed into the bulb's neck, the bulb is pumped through the exhaust tube, and the exhaust tube is melted shut.

The envelope of a lamp or valve has three parts: the bulb, the stem carrying the wires, and the exhaust tube for pumping.

  1. Flare: open one end of a 3–4 cm piece of 12–15 mm tubing into a trumpet as wide as the bulb's neck, with a carbon reamer.
  2. Assemble: stand the flare upright; inside it, a 5–6 mm exhaust tube and the lead-in wires — two for a lamp, three to nine for a valve — spaced round it.
  3. Press: heat the narrow top of the flare with the exhaust tube and wires until soft, and squeeze flat with heated brass or carbon pinch jaws, burying the wires in a press 6–10 mm high.
  4. Blow out: while the press is soft, blow sharply down the exhaust tube so a small hole bursts through into the future envelope. Anneal and inspect the stem.
  5. Mount the filament or electrodes on the leads (The Light Bulb, The Vacuum Tube).
  6. Seal in: slip the stem into the bulb so the flare's rim meets the neck, and turn it in the flame until neck and flare fuse all round. Pull off surplus glass and blow gently to smooth the seal. Anneal.
  7. Pump through the exhaust tube while baking the envelope below its strain point — soft glass to 350–400 °C, borosilicate to 450 °C (The Vacuum Pump).
  8. Tip off: heat the exhaust tube near the bulb with a small sharp flame until air pressure collapses it, and draw it off into a sealed tip.

Neon sign tubes are bent from soft or lead glass 8–15 mm across. Draw the lettering full size in reverse and lay glass-fibre cloth over it so you can bend face down. Heat a length on the ribbon burner — about one and a half tube widths for a sharp corner — bend it in the air, lay it on the pattern at once, and blow gently through the blow hose to restore full roundness; a flat bend makes a dark spot. Keep all bends in one plane, join runs with butt seals, and seal on electrodes and a pumping tube (Arc Lamps, Neon and Fluorescent Lights).

How to tell it worked

  • Polariscope: annealed glass stays dark between crossed polarisers; colours at a joint mean strain — re-anneal.
  • Joins: no line, ring, bubble or thin spot; the wall looks even when you sight along the tube.
  • Seal colours, seen through the glass:
Seal Good Bad
Platinum Bright metal, no bubbles Silvery thread or bubbles along the wire
Dumet Golden-copper to brick red Bright copper (no oxide) or black (too much)
Tungsten Golden-amber to copper-brown Silver (not wetted) or grey-black (burnt)
Housekeeper copper Clear red Black or brown: overheated
Kovar Mouse-grey to grey-brown Black and crusty
  • Spark test: on the pump, play the electrode of an The Induction Coil over every joint; a pinhole shows as a bright spark jumping into the glass.
  • Vacuum test: a week after sealing, a glow-discharge test should look the same as on the first day (The Vacuum Pump).
  • Thermal cycling: heat sealed pieces to 300 °C and back three times. Bad seals crack.

Note Troubleshooting. Join cracks minutes after making → not annealed, or glasses mixed — check with a thread test. Ring seal cracks → too thick, or the inner tube cooled first; thinner seal, anneal at once. Wire seal leaks → wrong oxide colour, or wire too thick. Lead glass turns black → reducing flame turned lead oxide to lead; add air. Bubbles in the joint → dirty glass or too hot a flame; wash and dry tubing first.

Dangers

Danger Eye damage. Hot soft glass gives a blinding yellow sodium flare, and every hot flame gives infrared that clouds the eye's lens over years — glassblower's cataract. Wear didymium glasses for soft glass (they filter out the yellow; didymium is a mix of the rare earths neodymium and praseodymium, Rare Earths, Cerium and Phosphors), and a welding shade 3–5 for borosilicate and quartz in oxygen flames.

Danger Oxygen and implosion. Oil or grease meeting pure oxygen can burst into fierce flame: keep oxygen fittings clean and dry, use flashback arrestors, light the gas first and turn off the oxygen first. Evacuated envelopes can implode and throw glass: wear eye protection and cage large ones in wire mesh.

  • Hot glass looks cold (Laboratory Glassware); rest finished pieces in one fixed "hot spot".
  • Spark testing. The induction coil gives tens of thousands of volts. Hold its electrode only by an insulated handle, keep your other hand away from the pump and frame, and do not linger on thin glass: the spark can punch a hole through it.
  • Sodium nitrite is poisonous and a strong oxidiser. Lead glass gives off lead fume when overheated: ventilate and wash hands (Lead).
  • Asbestos, once used for mats and gloves, causes cancer: use glass-fibre cloth, kaolin board or carbon.

Going further

How it was first done

Lampworkers in Venice and France shaped tubing over bellows-blown oil lamps in the 1600s. Thermometer makers of the 1700s and the Thuringian glassblowers after them made it a precise trade; Heinrich Geissler of Bonn sealed platinum wires through soft glass in his glowing discharge tubes from 1857. Swan's and Edison's lamps of 1879–1880 used platinum lead-ins, and its price drove the search for substitutes: Charles-Édouard Guillaume's iron–nickel "platinite" in the 1890s, and around 1911–1913 the copper-clad "dumet" wire worked out at General Electric, still in every ordinary lamp. Borosilicate glasses from Otto Schott in Jena and from Corning made hard-glass apparatus and tungsten seals possible. William Housekeeper of Western Electric published his knife-edged copper seal in 1923, and Howard Scott developed Kovar at Westinghouse around 1929–1936.

Source: content/entries/earth/scientific-glassblowing.md