Part 3 · Metals
The Blacksmith's Tooling
The tools a smith makes for the forge itself — tongs shaped for each job, the hardy and pritchel tools that sit in the anvil, top and bottom fullers, swages and the cast-iron swage block, flatters and set hammers, heading tools for nails and bolts, and mandrels and cones for rings — what each does, how to forge and harden it, and how to tell a good one.
- Difficulty
- ●●●●●
- Time
- An hour or two for a pair of tongs or a hardy once you are practised; a day for a set of top and bottom tools; a week to pattern, mould and cast a swage block or a cone mandrel
- Steps from zero
- 13 prerequisites →
This unlocks
—The full path from nothing — 13 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Hunting and Trapping
- Basic Woodworking
- Charcoal
- Hides and Leather
- Bellows
- Iron (the Bloomery)
- Blacksmithing
- Steel
- The Blacksmith's Tooling
Do them roughly in this order. See it on the tech tree →
Why it matters
A smith with only a hammer and an anvil can make almost anything, slowly. With the right tongs, a hardy, fullers and swages, the same job takes a third of the time and comes out truer. Smiths make these tools themselves: they are the first real projects after Blacksmithing, and each one puts a particular shape — a groove, a round, a shoulder, a flat face, a head — onto hot iron quickly and the same every time. They lead straight on to nails and bolts (Nails, Rivets and Wire Fasteners), tools (Axes, Chisels, Knives and Planes, Hammers, Pliers, Wrenches and Screwdrivers, Planes, Drawknives and Woodworkers' Tools), tube and pipe (Metal Pipes and Tubes), chain, hinges and wheel tyres (Wagons and Carriages).
How it works
Top and bottom tools. Most of these come in pairs. A bottom tool has a square shank that drops into the anvil's square hardy hole, so it stands firm on the anvil face. A top tool has a handle and is held on the work by the smith while a striker — a helper with a sledgehammer — hits it. The hot bar goes between them. A round-edged pair makes a groove (fullers), a half-round pair makes a round bar (swages), a flat-faced top tool smooths (flatter). With no striker, a smith uses the bottom tool alone and hits the work with the hand hammer.
The anvil's holes. A forged or cast anvil (Anvils, Trip Hammers and Power Hammers) has two holes through its heel: the square hardy hole, about 25 mm square on an anvil of 70–120 kg (19 mm on small anvils, 32 mm on big ones), and a round pritchel hole about 12–16 mm across. Make all your shanks to fit your own anvil. On a stone anvil (Blacksmithing), set a hardwood block or a thick iron plate with a square hole beside it to take the shanks.
Steel for hot tools. A tool that touches red-hot iron is heated by it. It must be tough rather than glass-hard, or it chips; and a hard edge is soon drawn soft by the work anyway. Use medium-carbon steel (about 0.5–0.8 % carbon; a file or wagon spring is about right — Steel), harden only the working face, and temper it to a blue (about 300 °C). Cool the tool in water every few blows while you use it. Struck ends are left soft and chamfered.
Handles for struck tools must not pass the blow into the hand: twist a green hazel rod round a groove in the tool, or fit a hardwood handle snugly but not wedged hard in an eye.
| Tool | Steel | Temper |
|---|---|---|
| Tongs | Mild (low-carbon) iron or steel | Not hardened |
| Hardy, hot chisels, punches | Medium-carbon | Edge or tip blue |
| Fullers, swages, flatters, set hammers | Medium-carbon | Face light blue; struck end soft |
| Heading tools | Medium-carbon | Around the hole blue |
| Swage block, cone mandrel | Grey cast iron | As cast |
What you need
- A working forge and anvil with hardy and pritchel holes, a hand hammer of 0.8–1.2 kg, a 3–5 kg sledgehammer for the striker, and your first tongs, punch and hot chisel (Blacksmithing).
- Stock: mild iron bar 12–20 mm square or round for tongs; medium-carbon steel bar 25–40 mm square for top and bottom tools; plate 12–15 mm thick for heading tools.
- Files, a grindstone, a quench tub of water and a small tub of oil (Files and Saws, Abrasives and Grinding Stones).
- For cast tools: a pattern, moulding sand and a cupola or crucible of grey iron (Metal Casting, The Blast Furnace and Cast Iron).
- Hazel, ash or hickory for handles.
- A striker, for the big top tools.
Where to find it
Iron and steel come from Iron (the Bloomery), Steel and Steel in Quantity. Old cart springs, files, axle steel and plough shares are good medium-carbon steel when you can find them, but you can carburise your own (Steel). Hazel grows as a multi-stemmed shrub in hedges and woodland edges, with round, toothed, soft-haired leaves and catkins in late winter; its straight shoots, cut in winter and used green, twist round a tool without cracking. Charcoal or coal fuel the forge (Charcoal, Coal and Coke).
Tongs for each job
Good tongs hold the work so firmly that you can hammer and turn it without it twisting or flying out; bad tongs drop hot iron on your foot. A working smith keeps twenty or more pairs, one for each size of stock. Your first pair is in Blacksmithing.
Proportions for tongs holding 12–20 mm stock: jaws 50–75 mm long; the boss (the flattened pivot section) 30–35 mm wide and about half the bar's thickness; reins 350–450 mm long and 10–12 mm thick, tapering slightly; rivet 8–10 mm. Longer reins give more grip and keep your hand further from the fire; heavier work needs heavier tongs.
Making a pair of flat tongs from 16–20 mm square mild bar:
- Jaw. Flatten 50–70 mm of the end over the anvil's edge into a jaw about 8 mm thick.
- Boss. Turn the bar 90° and flatten the next 30–35 mm, offset to one side, with a sharp shoulder between jaw and boss.
- Rein. Turn back 90° and draw the rest into a tapering rein 10–12 mm thick, or forge-weld on a rod (Blacksmithing).
- Make the second half to match the first.
- Rivet the bosses together with a red-hot rivet, and work the reins open and shut while hot until they move freely.
- Fit the hot jaws by closing them hard on a piece of the actual stock and hammering them to it. Gripping the stock, the reins should be 1–2 cm apart — never touching.
Patterns, made the same way with different jaws:
| Pattern | Jaws | Holds |
|---|---|---|
| Flat | Plain flat | Flat bar and plate |
| V-bit | A V-groove along each jaw | Round and square bar, gripped on four lines |
| Box (square-bit) | Turned-up sides making a channel | Flat bar that must not slip sideways |
| Bolt | Jaws bowed outward behind the tips | Bars with a head or a lump on the end |
| Pick-up | Long, bent, pointed tips | Picking small pieces out of the fire or tub |
| Scrolling | Narrow, round, short | Small scrolls and rings |
| Hollow-bit | Half-round groove | Round bar, rivets, punch blanks |
Shape grooves in jaws by forging them hot over a round bar or into a swage, not by filing.
A tong ring — a small oval link of 8–10 mm bar, slid over the reins — locks them closed on the work so you only need one hand for the tongs and the other for the hammer.
Good tongs: grip the work at the front and the back of the jaw, not just at the tips; you can twist the work hard against the hardy and it does not turn. Bad tongs: grip only at the tips (the work pivots), reins that touch, or a rivet so loose the jaws wobble sideways.
The hardy and other bottom tools
The hardy
A chisel edge standing upright in the hardy hole. Lay a hot bar across it and hit the bar with the hammer: the hardy cuts it from below. Nick a bar on four sides and snap it; cut nail rod to length (Nails, Rivets and Wire Fasteners).
- Take medium-carbon steel bar about 40 × 25 mm, or upset a 25 mm square bar.
- Shank. Draw one end to fit the hardy hole: square, parallel, slightly loose — it must drop in and lift out freely, and must not wedge. Length about 50 mm, so it does not reach the floor of the stump below.
- Shoulder. Leave a wide shoulder where shank meets tool so the tool sits firmly on the anvil face and does not ride down into the hole.
- Edge. Forge the top into a wedge 40–50 mm long, edge 30–35° included, standing 40–60 mm above the face. Grind the edge straight and slightly rounded at the corners.
- Harden the edge only, temper to blue.
Never strike the hardy's edge with the hammer: stop just short as the bar parts. A cold hardy, with a 50–60° edge hardened harder, cuts cold bar; never use a hot hardy cold.
The pritchel and its tools
The round pritchel hole is a backing hole: punch over it and the slug drops through. A pritchel is also a long, slim punch, 10–12 mm across tapering to the size of a horseshoe nail's shank, used to open nail holes in horseshoes over that hole. Draw it out of 12–15 mm medium-carbon steel, 250–300 mm long, temper the tip blue.
Other bottom tools take the same shank: a bending fork (two pegs 30–40 mm apart) for scrolls and hooks, a bick (a small pointed horn) for small rings on a horn-less stone anvil, and the bottom fullers and swages below.
Fullers
A fuller is a blunt, round-edged chisel. Driven into hot iron it makes a groove, pushing metal out to both sides. Use it to neck a bar before drawing a tenon, tang or rein, so the shoulder is crisp; to draw out fast (a row of grooves hammered flat lengthens a bar far quicker than the hammer face); and to spread a bar into a blade, spoon or shovel.
Sizes: keep fullers with edge radii of about 6, 10 and 13 mm; the bottom fuller of each pair matches its top fuller.
Bottom fuller: a hardy-shank tool with a rounded ridge on top, forged from solid or with a round bar forge-welded on. Top fuller: a block 30–40 mm square and 100–120 mm long, rounded at the bottom, with a chamfered striking face and a handle 400–500 mm long.
The spring fuller lets one person use both: a U of spring steel 3–4 mm thick with a top fuller on one arm and a bottom fuller on the other, held in the hardy hole. Slip the bar between and hammer the top. Make a spring swage the same way.
Swages and the swage block
A swage is a pair of tools, top and bottom, each with a half-round groove. Close them on a hot bar, hit, turn the bar a little, hit again: it comes out perfectly round, smooth and of exact size. Use them to finish round bar, tool handles, bolts, rivets, chain rod, axles, and for Iron and Brass Wire blanks.
- Make the groove radius the finished radius plus 1–2 %: hot bar shrinks as it cools.
- Leave a gap of 2–3 mm between the tools when closed on the bar, so they do not pinch a fin; make each groove a little less than a half-circle, with flared ends.
- Form grooves by forging the hot tool over a round bar of the right size, then file smooth. Square, hexagonal and V swages are made the same way.
The swage block
A swage block puts dozens of bottom tools in one heavy lump. A common size is 30 × 30 × 9 cm, weighing about 50–60 kg: round notches from 6 to 50 mm, V notches and square notches round all four edges; round and square holes through the face for heading, punching and bending; and a shallow dish 15–20 cm across and 3–4 cm deep on one face for doming spoons, ladles and bowls (Pots, Pans and Kettles).
It is cast in grey iron, not forged:
- Pattern in wood, 1 % oversize, with draft on every face; cores form the through-holes (Metal Casting).
- Mould it in green sand with risers over the thick parts, and pour about 70 kg of grey iron from a cupola (The Blast Furnace and Cast Iron) in one steady pour.
- Cool it in the sand at least a day; dress the notches with file and grinder.
- Stand: a stump or iron frame that holds it on edge at anvil height, or flat.
Until you can cast, make the most used notches as separate bottom swages.
Flatters and set hammers
Both are struck top tools with flat faces, held on the work while the striker hits.
- The flatter smooths. Its face is 50–75 mm square, perfectly flat, with the edges rounded to a radius of 3–5 mm so it leaves no marks. Pass it along a bar after drawing out to take out the hammer marks; a sheet or plate flattened under it comes out smooth enough to need little filing.
- The set hammer sets down shoulders and corners. Its face is smaller, 25–40 mm square, with sharp edges on at least one side. Set it on the work at the shoulder line and strike: it forms a crisp step, a square inside corner, or a tenon that a hand hammer could never reach.
Making: forge a medium-carbon steel block 50–75 mm square and 90–120 mm long, punch and drift an eye a third of the way from the struck end (Blacksmithing), and file the face flat to a straightedge. Chamfer the struck end 3–5 mm. Quench only the bottom 15–20 mm, let the heat run back until the face shows light blue, then quench all over. Fit a handle 400–500 mm long. Grind back any mushrooming of the struck end at once (see Dangers).
Heading tools
A heading tool (header) holds a bar upright while you hammer down its top to make a head — on a nail, a rivet, a bolt or a hook.
The nail header: a bar of medium-carbon steel about 25 × 12 mm, 250–300 mm long, swelled in the middle to 40 mm wide where the hole is. The hole is tapered: exactly the size of the nail shank at the top, 1–2 mm larger at the bottom, so the finished nail drops out when you tap it. Some headers have a second hole of a different size at the other end, or a domed top face to form a rosehead. Use is described in Nails, Rivets and Wire Fasteners.
The bolt header: a heavier plate 15–20 mm thick with holes of 6, 8, 10, 12 and 16 mm, used over the pritchel hole or an open stand; the bar is upset and its head forged down and squared or hexed on the plate, then finished in a cupping tool or a hexagon swage (Screws, Nuts and Bolts).
Making:
- Forge the bar and swell the hole area by upsetting or by forge-welding on a pad.
- Punch the hole from the top at a bright yellow heat, slightly undersize, flip, and punch through.
- Drift it to size with a tapered drift whose taper matches the one you want: drive it in from the bottom only, so the hole ends up wider below.
- File the top edge of the hole sharp and the top face flat.
- Harden the area round the hole and temper it to blue.
Good one: the hole is square to the face and the nail falls out with a tap. If the hole is wider at the top, the nail jams.
Mandrels and cones
A mandrel is any shape that hot metal is forged around. Small ones are tapered round or square bars held in the vice or the hardy hole: a drift to open an eye to size, a tapered bar to forge rings and hooks.
The cone mandrel is the big one: a hollow cast-iron cone 60–100 cm tall, about 25–35 cm across at the base and 3–5 cm at the tip, often with a groove down one side so a ring with a lump or a hook on it can still slide down. It stands on the floor beside the anvil. Drop a forged ring over it and hammer the ring down: it comes out truly round. Hammer it further down and it stretches to a bigger size. Use it for rings, collars, hoops, ferrules, cart wheel bands (Wagons and Carriages) and barrel hoops (Barrels and Cooperage).
Making: turn a wooden pattern on the The Lathe, 1 % oversize, with a core to make it hollow (a solid cone is needlessly heavy), and cast it in grey iron as for the swage block. A small forged cone for rings up to 10 cm: taper a round bar 50 mm thick over a length of 300 mm down to 15 mm, and fit a square shank on the big end for the hardy hole or the vice.
How to tell it worked
- Tongs hold a bar so firmly that you can hammer it on its edge and twist it against the hardy without it moving in the jaws.
- The hardy cuts a 20 mm bar at yellow heat in four to six blows and its edge is unharmed afterwards.
- Fullers and swages leave smooth, even grooves and round bars with no fins; a swaged bar fits a ring gauge at every point along its length.
- The flatter leaves a surface with no hammer marks.
- Headers release the finished nail or bolt with one tap.
- The cone makes rings that sit flat on the anvil face all round and pass a template.
- No tool chips, cracks or bends after a day's use. If one does, it was too hard or too soft — see below.
Note Troubleshooting. Tongs let the work twist → jaws touch only at the tips; reheat and refit them to the stock. Reins touch → close the jaws a little more, or open the reins hot. Hardy wedges in the hole, or wobbles → shank too big or too small; it should drop in freely and sit on its shoulder. Top tool edge or face chips → too hard; temper further, to full blue. Face dents and spreads → too soft; reharden. Fuller or swage leaves a fin along the bar → tools closing too far, or the bar not turned enough between blows. Nail jams in the header → hole tapers the wrong way; re-drift from below. Cast swage block cracks on cooling → thick and thin parts cooled unevenly; leave it in the sand longer and make the pattern more even in thickness.
Dangers
Danger Mushroomed heads throw steel splinters. Every struck tool — punches, chisels, fullers, set hammers, flatters — spreads at its struck end with use. The ragged edge can break off under a sledge blow and fly out like a bullet, into an eye, a throat or a hand. Grind struck ends back to a smooth chamfer as soon as they start to spread. Never strike one hardened tool with another hardened face; never strike a hardy or an anvil face with a sledge.
Warning Working with a striker. A 4 kg sledge swung by someone who cannot see where it will land can break the holder's hand. Agree signals before starting: the smith taps where to hit and how hard, the striker hits only where the smith's hammer has just tapped, and stops the instant the smith's hammer goes quiet or the smith says "stop". Keep the tool-holding hand well back on the handle, never near the head. Strikers stand square to the anvil and never swing over their head with a slippery handle.
- Falling work. Hot iron dropped from slipping tongs burns through boots: use tongs that fit, a tong ring, leather boots and apron.
- The hardy is a blade at waist height: take it out of the hole when not in use.
- Pouring cast iron: see Metal Casting.
What this unlocks
With a full set of tooling, a smith can make nails and bolts by the thousand (Nails, Rivets and Wire Fasteners, Screws, Nuts and Bolts), chain and rings, hinges and hasps (Doors, Hinges, Handles and Latches, Locks and Keys), cooking pots and ladles (Pots, Pans and Kettles), tools of every kind (Axes, Chisels, Knives and Planes, Hammers, Pliers, Wrenches and Screwdrivers, Planes, Drawknives and Woodworkers' Tools), wheel tyres and wagon ironwork (Wagons and Carriages) and horseshoes (Draft Animals and Harness). The same top-and-bottom idea, scaled up and driven by water or steam, becomes the power hammer, the drop forge and closed-die forging (Anvils, Trip Hammers and Power Hammers, Presses, Punches and Dies), the basis of Precision and Interchangeable Parts.
How it was first done
The earliest smiths held hot metal with green sticks and stones; hinged tongs much like modern ones appear in Greek vase paintings of the god Hephaestus's forge, and Roman sites across Europe have yielded tongs, hot sets, fullers and nail headers in forms a modern smith would recognise. A Viking-age tool chest found at Mästermyr on the Swedish island of Gotland, probably from around AD 1000, held smith's and carpenter's tools including anvils, several pairs of tongs, hammers, shears, a draw plate and files.
Swage blocks became common once cheap cast iron was available in the 18th and 19th centuries, and the specialist tongs, fullers, flatters and set hammers of the 1800s were shown in detail in the smithing manuals of that time. James Nasmyth's steam hammer of the late 1830s and the drop hammers of the following decades scaled the same top-and-bottom tools up to forge ship shafts, railway axles and gun parts, and closed-die drop forging became the method for mass-produced spanners, wrenches and engine parts.
Source: content/entries/metals/blacksmiths-tooling.md