◆ Rebuild

Part 3 · Metals

Blacksmithing

Heat iron until it glows and shape it with a hammer. Build a clay forge, use a stone as your first anvil, read the metal's temperature by its colour, and make your first punch, tongs, hammer and knife.

Difficulty
●●●●●
Time
Two days to build a forge; years to master, but a punch or a knife on your first day
Steps from zero
11 prerequisites →

You need first

Iron (the Bloomery)

This unlocks

Doors, Hinges, Handles and LatchesCopper WireSpades, Hoes, Rakes and WheelbarrowsTroughs, Separators and Livestock GearSeed Drill and ReaperBarrels and CooperageKitchen and CookingLocks and KeysThe Steam EngineAnvils, Trip Hammers and Power HammersThe Blacksmith's ToolingHammers, Pliers, Wrenches and ScrewdriversNails, Rivets and Wire FastenersScissors, Shears and Folding KnivesSheet Metal and RollingSteelIron and Brass WireBits, Stirrups and Spurs
The full path from nothing — 11 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing

Do them roughly in this order. See it on the tech tree →

Why it matters

A bloom from the Iron (the Bloomery) furnace is just a lump. The blacksmith turns it into everything else: nails, hinges, axes, hoes, sickles, chisels, knives, chains, hooks, wedges, rivets, cooking pots, horseshoes, and the tools to make better tools. Iron does not cast in a simple furnace — it has to be forged, heated until it is soft and then hammered into shape. That is the skill in this chapter.

Blacksmithing is also where you make the tools every other craft needs: the axes and adzes for Basic Woodworking, the plough points for the The Plough, the punches and drawplates for Copper Wire, the parts of the The Lathe and the The Steam Engine. Once you can forge-weld, you can join pieces into any size you need. Once you can make Steel, your edges will be harder than anything before.

How it works

Iron is stiff when cold, but as it heats it softens. At a bright orange heat (about 1,000 °C; see Materials Data Tables) it moves under the hammer like stiff clay. Below a dull red heat it becomes stiff again, and hammering it then can crack it. So a smith works in short bursts — heat, hammer for a few seconds, reheat — and reads the temperature from the colour of the glow.

Too coldstop forging Hardensteel Forgemain working heat Weldstar sparks faint reddull redblood redcherrybright cherryorangeyellowlight yellowwhite 500 °C6007008009001,0001,1001,2001,300 Judge colours in shade. In bright sunlight every colour looks one step colder than it is.
Fig. 1 Heat colours of iron, seen in shade. Do your heavy forging from yellow to orange; stop when it fades to red.
Colour (seen in shade) Temperature What it means
No glow, but sizzles water 100–450 °C Black heat. Looks cold, burns to the bone.
Faint red, visible only in the dark 500–550 °C Too cold to forge.
Dull "blood" red 600–700 °C Stop forging iron. Light finishing blows only.
Cherry red 750–800 °C Hardening heat for steel (see Steel).
Bright cherry to orange 850–950 °C Light forging; bending.
Orange to yellow 1,000–1,150 °C Main forging heat. The metal moves easily.
Light yellow to white, sparkling 1,250–1,350 °C Welding heat. A few bright star-sparks.
Fizzing white with many sparks above 1,350 °C Burning. The iron is being destroyed. Pull it out.

Always judge colours in the shade — under a roof or with your back to the sun. In bright sunlight, a hot bar can look almost cold.

Two other facts matter:

  • Scale. Hot iron reacts with air and grows a black skin of iron oxide called scale, which flakes off under the hammer. Every heat costs a little metal. Brush it off with a stick or a bundle of twigs before hammering, so it is not driven into the surface.
  • Where the heat is. In front of the tuyere, the air blast is full of oxygen and burns the metal. A little higher, above the tuyere and covered with charcoal, the fire is hot but starved of oxygen — that is where the iron should sit. Keep a mound of charcoal over the work.

What you need

Item Notes
Forge A clay hearth with a tuyere, below
Bellows A pair of bag or pot bellows, or a hinged bellows. See Bellows.
Charcoal Broken to 1–3 cm — finger-joint size. About 5–10 kg for a day's work. See Charcoal.
Anvil A big flat-topped hard stone to begin with, below
Hammer A hafted stone hammer to begin with; an iron one as your first project
Tongs Green-wood tongs to begin; iron tongs soon after
Quench bucket Water, for cooling tools and tongs — kept to one side
Iron Bar iron from consolidated blooms (see Iron (the Bloomery))
Fine dry sand As welding flux

Building the forge

A side-blast forge is a clay box at waist height with a hollow for the fire and the tuyere coming in from the side.

Fire wallshields the bellows Firepot under a charcoal mound25–30 cm wide, 12–15 cm deep one step 75 cmhip height Bellows Tuyere8–10 cm abovefirepot floor Anvil stoneface at knuckleheight Hardwoodstump quench water
Fig. 2 A side-blast forge and anvil. The fire sits in a hollow at waist height; the anvil face is at knuckle height, within one step of the fire.
  1. Build the base of stones and clay, or a box of logs filled with earth, about 75 cm high (hip height), with a top about 80 × 60 cm.
  2. Make the hearth. Cover the top with 10 cm of the clay-sand-straw mix used for furnaces (see Iron (the Bloomery)). In the middle, form a round hollow — the firepot — about 25–30 cm across and 12–15 cm deep.
  3. Build the fire wall. On the bellows side, raise a clay wall 30 cm high and 10 cm thick. It shields the bellows and holds the tuyere.
  4. Set the tuyere through the wall so it enters the firepot 8–10 cm above its bottom, pointing horizontally or a little down. Keep the tip flush with the wall of the firepot, not sticking out, so it doesn't burn away.
  5. Dry the forge slowly for several days, then with small fires.

The simplest of all forges is a ground forge: a hollow in the earth with a tuyere coming in from the side and the bellows behind it. Smiths in Africa and Asia have worked kneeling or sitting at such forges for thousands of years. It works perfectly well; it is just harder on your back.

Running the fire. Light kindling in the firepot, cover it with charcoal and start the bellows gently. Heap charcoal over the top so the fire is a mound 15 cm high. Push the iron into the heart of the mound, just above the level of the tuyere, and cover it. Blow steadily. A bar 1–2 cm thick reaches forging heat in 2–5 minutes. If the fire spreads too wide, rake charcoal back toward the middle.

The anvil

To start, find a hard, tough, flat-topped stone of 20–50 kg: basalt, granite, diorite or quartzite, without cracks (strike it with a hammerstone — a good one rings; a cracked one sounds dull). A smooth river boulder with a broad flat face is ideal. A second, rounded stone helps with bending and making curves.

Set it in a hole in the ground or on a hardwood stump so that its face is at your knuckle height when you stand beside it with your arm hanging straight. Place it one step from the forge, on your hammer-hand side.

Later, weld several blooms together into an iron block for a real anvil, or make one from The Blast Furnace and Cast Iron (see Anvils, Trip Hammers and Power Hammers).

Your first hammer and tongs

Stone hammer. Pick a tough, rounded, fist-sized stone (0.6–1 kg) and peck a groove round its waist with a harder stone. Bend a split green hardwood handle round the groove and bind it tightly with wet rawhide, which shrinks hard as it dries (see Stone Tools).

Green-wood tongs. Split one end of a green sapling 3 cm thick for 20 cm, tie a binding behind the split, and wedge the jaws apart with a pebble. They hold small hot pieces for a few heats before they char. Soak them in water between heats.

Work from a long bar. Even easier: forge on the end of a bar long enough that you can hold the other end in your bare hand. Iron conducts heat slowly. A bar 60 cm long stays cool at the far end for several minutes. Make the object on the end, then cut it off. Smiths have always done this.

Iron tongs — your first real project. Make two identical halves from a bar about 12 mm square and 45 cm long. For each half, flatten the first 5 cm into a jaw, flatten the next 3 cm at 90° into a round boss, and draw the rest out into a long rein. Punch a hole through each boss, put the halves together and set a hot iron rivet through both. Work the joint while it is hot until the tongs open and close freely, then shape the jaws to fit your bar.

The basic operations

longer thicker at the hot end slug punch sparks Drawing outturn 90° every few blows Upsettingheat only the end Punching¾ through, flip, punch out Forge weldingscarfed ends, white heat
Fig. 3 The four basic operations. Almost everything a smith makes is a combination of these.

Drawing out (making longer and thinner)

  1. Heat to orange-yellow.
  2. Hammer the bar near the edge of the anvil, along the part you want thinner, with firm overlapping blows.
  3. Turn the bar a quarter turn (90°) after every few blows, so it stays square. Hammer it square first, then knock off the corners to make it eight-sided, then round it.
  4. To draw faster, hammer over a rounded stone or the edge of the anvil: the narrow contact pushes the metal lengthways instead of sideways.

Upsetting (making shorter and thicker)

  1. Heat only the end you want to thicken. If the whole bar is hot, dip all but the end in water.
  2. Stand the bar on end on the anvil, hot end down, and hammer the cold end straight down. Or hold it level and ram the hot end against the anvil.
  3. If it starts to bend, straighten it before continuing. Upsetting is slow; it takes many heats.

Bending

Heat the place you want to bend to bright orange, then bend it over the edge of the anvil, around the rounded stone, or between two pegs driven into a hardwood stump. Heat only the place you want to bend.

Punching

  1. Heat to bright yellow.
  2. Set a punch (see below) where you want the hole and hit it hard. Drive it three-quarters of the way through.
  3. Cool the punch in water after every few blows, or it will soften and mushroom.
  4. Turn the piece over. You will see a dark spot where the punch has nearly come through. Punch through from this side over a gap (a hole in a stone, or between two stones) and the small plug — the slug — drops out.
  5. Enlarge or round the hole by driving a tapered bar (a drift) through it.

Cutting

Cut hot metal with a hot chisel: a chisel with a 30–40° edge. Heat the bar to yellow, put it on the anvil, and drive the chisel halfway through. Turn the bar over and cut from the other side. Never cut right through onto your stone anvil — it ruins the chisel edge. Stop just short and snap the bar over the edge.

Forge welding (joining two pieces into one)

Bloom iron welds very readily — this is how you build up larger pieces, and how you add a steel edge to an iron tool.

  1. Scarf the ends. Hammer each end into a short, tapered, slightly rounded wedge (a scarf), so that the two pieces overlap by 2–3 times the bar's thickness.
  2. Clean the fire. Remove ash and slag lumps. Build a deep mound of fresh charcoal over the tuyere.
  3. Heat slowly to bright yellow. Sprinkle fine dry sand on the scarfs. The sand melts into a glassy coat — a flux — that dissolves scale and keeps air off the surface.
  4. Bring to welding heat. Blow harder until both pieces look light yellow to white, wet and shiny, and the first few bright star-shaped sparks jump from the surface. Do not wait for heavy sparking — that is burning.
  5. Act fast. Take both pieces out, tap them on the anvil to knock off loose scale, lay one scarf on the other, and hit lightly first to stick them, then firmly to set the weld. You have only a few seconds.
  6. Reheat and hammer again at welding heat to make sure the joint is solid, then forge it to shape at normal heat.

Your first tools

A punch. Take a bar about 12 mm square and 15–20 cm long. Draw one end out into a long gentle taper ending in a flat tip 5–6 mm across. Round the striking end a little. That's all. (Hardened Steel punches last longer, but an iron punch works for hot punching if you cool it often.)

A hot chisel. From a bar 15–20 mm square and 20 cm long, flatten one end into a wedge 3 cm wide and grind or file the edge to 30–40°. Like the punch, it works only on hot metal.

An iron hammer. Take a block 3 × 3 × 9 cm (about 0.6–0.8 kg). Mark the middle, punch an eye through it from both sides with your punch, then drift it out to an oval about 2 × 3 cm. Dress the faces flat and slightly rounded at the edges. Fit a hardwood handle 30–35 cm long and wedge it tight.

A knife.

  1. Take a bar 4–6 mm thick and 2–3 cm wide.
  2. Forge the point: hammer the corner of the end down at an angle so it tapers to a point.
  3. Draw out a tang behind the blade length (10–15 cm), narrowing it to about 1 cm wide and 8 cm long to fit into a handle.
  4. Forge the bevel: hammer the edge side of the blade thinner, working on both faces, until the edge is about 1 mm thick. The blade will curve away from the edge as you do this; that is normal — pre-bend it slightly the opposite way first, or straighten it afterwards.
  5. Normalise: heat the whole blade evenly to cherry red and let it cool in the air. Do this three times. It relieves the stresses of forging.
  6. Grind the edge sharp on a sandstone slab or wheel, with water.
  7. Fit a wood or bone handle by heating the tang and burning it into a drilled hole.

A knife of plain bloom iron is soft. It will cut, but it dulls quickly. For a hard edge, it must be steel — see Steel for how to add carbon, harden and temper it.

How to tell it worked

  • Clean forging — the surface is smooth, without cracks, folds or flaps of metal.
  • The weld test. Clamp a welded test bar with one end in a crack in a log and bend it sharply across the weld while hot. A good weld bends with the bar. A bad weld opens up along the joint.
  • Even colour. A piece heated evenly bends evenly. A bar that bends in only one spot was heated in only one spot.

Note Troubleshooting. Metal cracks at the edges while hammering → too cold. Stop at dull red. If bloom iron cracks even when hot, it may contain sulfur; if it is brittle only when cold, it may contain phosphorus (common in bog iron) — still fine for many tools but not for springs or hammered blades. Weld won't stick → not hot enough, dirty fire, or too slow from fire to anvil. Clean the fire, flux, and move faster. Surface eaten away, crumbly and sparkling → burnt iron. It was in the direct blast or left too long at white heat. Cut off the damaged part. Fire keeps dying → ash and slag are blocking the tuyere. Clean out the firepot.

Dangers

Danger Black heat burns. Iron that has stopped glowing can still be 400 °C. Every piece of metal near a forge is hot until proved otherwise. Never pick up iron with your bare hand without first holding your palm near it, or flicking water on it to see if it sizzles. Put hot pieces down in one agreed place, never on the ground where others walk.

  • Carbon monoxide. Forges make it too. Work under an open-sided roof or outdoors.
  • Flying scale and sparks. Hot scale flies off with every blow. Protect your eyes — even a leather flap or squinting behind a raised hand helps — and wear leather or wool, never anything that melts.
  • Hammer and anvil injuries. Keep the anvil face flat and dry; a glancing blow sends the hammer, or the work, flying. Make sure the hammer head is wedged tight on its handle.
  • Hearing. Ringing blows on iron damage hearing over years. Plug your ears with soft wax and wool.
  • Burnt clothing and hair. Tie back hair; roll down sleeves.

What this unlocks

With forging and welding you can make nails, hinges, chains, hoes and axes, the workshop Hammers, Pliers, Wrenches and Screwdrivers, the special tongs, fullers and swages of The Blacksmith's Tooling, the tools for Basic Woodworking and the The Plough, drawplates for Copper Wire, and parts for the The Lathe, pumps and the The Steam Engine. The next step is to make the metal itself harder: Steel, for edges, Springs and Files and Saws.

How it was first done

Blacksmithing began as soon as people smelted iron, more than 3,000 years ago in Anatolia and the Near East, and independently or soon after in Africa and China. For most of history the smith was among the most important people in any village. Many smiths in Africa and India worked with stone anvils and ground-level forges, exactly as described here, until recent times. A complete Viking-age smith's tool chest, found at Mästermyr on the Swedish island of Gotland and dating from about AD 1000, held tongs, hammers, small anvils, punches, chisels and files remarkably like those of a village blacksmith of 1900 — the tools you will make in this chapter.