◆ Rebuild

Part 3 · Metals

Permanent Magnets

Why some materials hold their magnetism and others forget it, and how to make strong magnets on purpose — hardened magnet steels, cast alnico, ferrite ceramic magnets from iron oxide and barium or strontium, and rare-earth magnets in outline — then how to magnetise them, keep them and test them.

Difficulty
●●●●●
Time
An afternoon to harden and magnetise steel magnets; a day for an alnico melt and two days of heat treatment; about a week from raw oxide to a batch of ferrite magnets
Steps from zero
31 prerequisites →

You need first

MagnetsNickel and CobaltRare Earths, Cerium and Phosphors

This unlocks

Loudspeakers, Microphones and Headphones
The full path from nothing — 31 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. Charcoal
  10. Pottery
  11. The Kiln
  12. Hides and Leather
  13. Salt
  14. Lime
  15. Fermentation
  16. Lye and Potash
  17. Glass
  18. Bellows
  19. Acids, Bases and Testing
  20. Saltpeter
  21. Iron (the Bloomery)
  22. Copper Smelting
  23. Laboratory Glassware
  24. Sulfuric Acid
  25. Identifying Substances
  26. Nitric Acid
  27. Magnets
  28. The Battery
  29. Rare Earths, Cerium and Phosphors
  30. Electrolysis
  31. Nickel and Cobalt
  32. Permanent Magnets

Do them roughly in this order. See it on the tech tree →

Why it matters

A lodestone or a stroked needle (Magnets) is enough for a The Compass. But a motor, a The Generator, a The Telephone earpiece, a moving-coil meter (Measuring Electricity), a microphone or a loudspeaker (Loudspeakers, Microphones and Headphones) needs a magnet that is strong, stays strong, and is small. Better magnets mean a lighter magneto for an engine's spark (The Internal Combustion Engine), a bicycle dynamo that fits on a fork (The Bicycle), a fan motor that needs no field winding (Fans, Vacuum Cleaners and Washing Machines), a magnetic separator that pulls iron out of grain or ore (Mining and Tunnelling), a door catch, a fridge seal.

Over one century magnets grew about a hundred times stronger for the same size: hardened carbon steel, then tungsten and cobalt steels, then cast alnico in the 1930s, cheap ferrite in the 1950s, and rare-earth magnets from the 1970s. Each step is made from things this book has already rebuilt.

How it works

Every iron, nickel or cobalt material is made of tiny magnetic domains (Magnets). Magnetising lines them up. What makes a material a permanent magnet is how firmly they stay lined up afterwards.

Two numbers describe a magnet material:

  • Remanence — how strongly magnetised it stays after the magnetising field is removed. It sets how hard it can pull. Measured in tesla (T).
  • Coercivity — how strong a reverse field it takes to knock the magnetism out. It sets how well the magnet resists being weakened by its own shape, by knocks, by other magnets and by heat. Measured in kiloamperes per metre (kA/m). A coil makes a field of (turns × amperes) ÷ length in metres: 1,000 turns carrying 1 A over 1 m make 1 kA/m.

Soft iron has high remanence but almost no coercivity, so it forgets: good for The Electromagnet cores, useless as a magnet. A good magnet material has both. The product of the two, the energy product, is the best single measure of strength per volume.

Soft ironforgets at once Magnet steelremembers, weakly Alnicostrong pull, holds well Ferriteweaker pull, very stubborn remanencecoercivity magnetismfield from the coil → (loops not to scale: ferrite needs about 50 times the field of steel)
Fig. 1 Magnetising loops. As the field is raised and lowered, each material traces a loop. Where the loop crosses the upright axis is the remanence; where it crosses the level axis is the coercivity. Soft iron makes a tall, thin loop; magnet materials make wide ones.

What locks the domains. In quenched steel, carbon atoms trapped in a strained crystal (martensite, see Steel) pin the domain walls. In alnico, the metal splits during heat treatment into needles of iron-cobalt in a nickel-aluminium matrix, each needle too thin to hold more than one domain. In ferrite and rare-earth magnets, each crystal is so strongly magnetised along one direction that turning it needs an enormous field; ground to grains of about 1 µm, each grain is a single locked domain.

Shape matters. A magnet's own poles push back against its magnetism. The lower the coercivity, the longer and thinner it must be:

Material Remanence Coercivity Energy product Shape it needs Safe up to
Carbon steel, 1% C, quenched 0.9 T 4 kA/m 1.6 kJ/m³ Long: length 15–20 × thickness 100 °C
Tungsten steel, 6% W 1.0 T 5.6 kA/m 2.5 kJ/m³ Long: 12–15 × 100 °C
Chrome steel, 3.5% Cr 0.95 T 5 kA/m 2.3 kJ/m³ Long: 12–15 × 100 °C
Cobalt steel, 35% Co 0.9 T 19 kA/m 8 kJ/m³ 5–8 × 150 °C
Alnico 2, cast 0.75 T 45 kA/m 13 kJ/m³ 3–5 × 450 °C
Alnico 5, cast in a field 1.25 T 50 kA/m 40 kJ/m³ 4–5 × along the set axis 500 °C
Ferrite, oriented 0.4 T 250 kA/m 30 kJ/m³ Short, flat: discs, rings, arcs 250 °C
Samarium–cobalt 0.9 T 700 kA/m 160 kJ/m³ Any 250–300 °C
Neodymium–iron–boron 1.2–1.4 T 900 kA/m 250–400 kJ/m³ Any 80–150 °C

Heat. Every magnet loses its magnetism at its Curie point — 770 °C for iron, about 860 °C for alnico, 450 °C for ferrite, about 320 °C for neodymium magnets — and weakens well before that.

Magnetic circuits. A magnet is used as part of a loop: the magnet, soft-iron pole pieces that lead its flux to where it is wanted, and an air gap where the work is done (where a coil moves or an armature turns). Keep the gap as short as possible: every extra millimetre of air costs strength.

What you need

Item For See
Crucible steel, tungsten, chromium, cobalt Magnet steels Alloy and Stainless Steels, Tungsten and Filament Wire, Chromium and Its Compounds, Nickel and Cobalt
Pure iron, nickel, cobalt, aluminium, copper Alnico Iron (the Bloomery), Nickel and Cobalt, Aluminium, Copper Smelting
Furnace reaching 1,650 °C Melting alnico The Electric Arc Furnace, Electric Kilns and Furnaces
Pure red iron oxide Ferrite Pigments, Paints and Varnish
Barium or strontium carbonate Ferrite The Vacuum Tube
Ball mill with steel balls Grinding ferrite to 1 µm Portland Cement
Press and hardened die Pressing ferrite Powder Metallurgy
Kiln to 1,250 °C Firing ferrite The Kiln
Large electromagnet, battery bank or dynamo Magnetising; field cooling of alnico The Electromagnet, The Rechargeable Battery, The Generator
Silicon carbide wheels Grinding alnico and ferrite Abrasives and Grinding Stones, Precision Grinding

Where to find it

Iron oxides — magnetite and hematite — and green vitriol (iron sulfate) are described in Finding and Identifying Ores and Sulfuric Acid. Barite (heavy white "heavy spar") and celestine (pale blue, also very heavy) occur in veins in limestone and with lead ores; see The Vacuum Tube for turning them into carbonates. Cobalt and nickel come from the ores in Nickel and Cobalt, tungsten from wolframite and scheelite (Tungsten and Filament Wire), chromium from chromite (Chromium and Its Compounds), and the rare earths from monazite and bastnaesite sand (Rare Earths, Cerium and Phosphors).

Method 1: Magnet steel

The easiest strong magnet. A steel horseshoe or bar, properly hardened and magnetised in a coil, is several times stronger than one stroked with a lodestone.

The steels

Steel Recipe (by weight) Harden from Quench in
Carbon 0.9–1.1% carbon 780–800 °C, cherry red Water or brine
Tungsten 5–6% tungsten, 0.6–0.7% carbon 820–850 °C Water
Chrome 2–3.5% chromium, 0.9–1% carbon 830–850 °C Oil or water
Cobalt (KS steel) 30–40% cobalt, 5–9% tungsten, 2–3% chromium, 0.7–0.9% carbon 950 °C Oil

Melt them in crucibles as in Alloy and Stainless Steels. Tungsten steel was the standard magnet steel for telephones and magnetos from the 1880s to the 1920s; cobalt steel was much better but costly.

Making a horseshoe magnet

  1. Forge a bar into a U, legs parallel, with the gap between the legs about equal to the bar's width. A useful size: bar 25 × 6 mm, legs 100 mm long. Keep the bar long and thin in proportion: a short, fat steel magnet weakens itself.
  2. Grind or file the pole faces flat and square, while the steel is soft.
  3. Harden. Heat the whole piece evenly to the temperature in the table — check with a lodestone or magnet: steel stops being attracted at about 770 °C, so heat just past that point, then a little more for alloy steels. Plunge it legs-first, straight down, and stir.
  4. Do not temper. Tempering weakens a magnet. Instead, age it: boil it in water for 5–10 hours. This relieves the worst strains so the magnet will not slowly lose strength in the first months.
  5. Magnetise (below), then fit a keeper across the poles at once.

Compound magnets. Thin steel hardens right through; thick steel does not. Instead of one thick horseshoe, harden several thin ones (3–6 mm) separately, magnetise each, and bolt them together side by side with like poles together, using brass bolts. The stack is stronger than one solid piece of the same size. Magnetos and early telephone receivers were built this way.

Method 2: Alnico

Alnico (aluminium, nickel, cobalt with iron) is cast, not forged. It is too hard and brittle to cut, so it is cast nearly to shape and finished only by grinding.

Recipes

Grade Aluminium Nickel Cobalt Copper Iron Notes
Alnico 2 10% 19% 13% 3% 55% No field needed; easier
Alnico 5 8% 14% 24% 3% 51% Must cool in a magnetic field; three times stronger
Nickel–aluminium (MK) steel 12% 25–30% — — rest No cobalt; weaker than alnico 2 but far better than any steel

Casting

  1. Melt the iron, nickel and cobalt first in a magnesia- or alumina-lined crucible in an arc or induction furnace (The Electric Arc Furnace, Electric Kilns and Furnaces). Alnico pours at about 1,600 °C, a dazzling white heat.
  2. Add copper, then aluminium last, in small pieces pushed under the surface with a rod. Aluminium burns and makes dross; add 0.5–1% extra to make up for it, skim, and pour at once.
  3. Pour into dry sand moulds bonded with oil or a little clay (Metal Casting), with large risers: alnico shrinks a lot and cracks if the mould holds it tightly. Cast holes in place; you cannot drill them later.
  4. Shake out while still hot and cool slowly in sand or ash.

Heat treatment

  1. Solution heat. Heat the castings to 1,250–1,300 °C for 15–30 minutes, in a closed box packed with charcoal or in hydrogen to limit scaling.
  2. Controlled cooling. For alnico 2, cool in still air to below 500 °C. For alnico 5, put each hot casting between the poles of a strong electromagnet — at least 120–160 kA/m along the direction you want the poles — and let it cool in the field, at roughly 1 °C a second through the range from 900 to 700 °C — about three minutes to cool through it. Slow a small casting by setting it in a thin fireclay sleeve or a loose wrap of Glass Fibre and Glass Wool; speed a big one with a gentle air blast. This lines up the needles that form, along the field. Cooled across the field, it will be weak in the wrong direction for ever.
  3. Age (draw) at about 590–600 °C for 8–20 hours, then cool in air.
  4. Grind to size with a silicon carbide wheel and plenty of water, a light cut at a time.

Sintered alnico. Small alnico parts can be pressed from mixed powders, using the aluminium as a brittle iron–aluminium alloy crushed to powder, and sintered at about 1,300 °C in very dry hydrogen (Powder Metallurgy). It is slightly weaker than cast, but accurate and strong.

Method 3: Ferrite (ceramic) magnets

1 Mix and calcine iron oxide SrCO₃ 6.3 : 1 by weight fire 1,200–1,300 °C, 1–2 h 2 Grind wet steel balls, 10–20 hours to grains of about 1 µm 3 Press in a field field coil 400–800 kA/m lines up the grains; water drains 4 Fire in air 1,180–1,250 °C, 1–2 h; shrinks about 15% 5 Grind to size silicon carbide or diamond, with water NS 6 Magnetise pulse coil, 800–1,000 kA/m
Fig. 2 Making ferrite magnets. Iron oxide and strontium or barium carbonate are mixed, fired into clinker, ground to a fine slurry, pressed in a magnetic field so every grain points the same way, fired again, ground to size and magnetised.

Ferrite magnets are a kind of pottery: a compound of iron oxide with barium or strontium oxide. They are weaker than alnico per kilogram but resist demagnetising far better, need no cobalt or nickel, do not rust, and cost little more than the iron oxide and kiln fuel. Most motors, loudspeakers and door catches in the world use them.

  1. Pure iron oxide. Roast green vitriol (iron sulfate) at 650–750 °C to a bright red powder, wash out the remaining sulfate with hot water and dry it (Pigments, Paints and Varnish). Or dissolve iron or scale in Hydrochloric Acid and precipitate it with soda, then roast. It must be free of sand: more than a few tenths of a percent of silica spoils the magnets.
  2. Barium or strontium carbonate from barite or celestine, as in The Vacuum Tube. Strontium makes slightly better magnets and is less poisonous.
  3. Weigh and mix. For strontium ferrite: 6.3 parts iron oxide to 1 part strontium carbonate by weight. For barium ferrite: 4.7 parts iron oxide to 1 part barium carbonate. (This is slightly less iron oxide than the formula, SrO·6Fe₂O₃, which helps.) Ball-mill wet for 2–4 hours to mix.
  4. Calcine. Dry the slurry and fire it in clay saggers at 1,200–1,300 °C for 1–2 hours. It reacts to a dark grey, hard clinker that is already magnetic.
  5. Grind fine. Crush, then ball-mill wet with hardened steel balls for 10–20 hours, until the grains are about 1 µm — so fine that the slurry feels like cream and a drop dried on glass shows no grit to a fingernail. This is the step that makes or breaks the magnet.
  6. Press. For simple isotropic magnets, dry the slurry, mix in 1% starch or gum arabic paste as binder, granulate through a sieve and press at about 0.5–1 t/cm² in a steel die (Powder Metallurgy). For oriented magnets — twice as strong — press the wet slurry (about two-thirds solids) in a non-magnetic die with an electromagnet around it giving 400–800 kA/m along the pressing direction. The grains turn to line up with the field. Water is squeezed out through filter paper or cloth over holes in the punch.
  7. Fire in air at 1,180–1,250 °C for 1–2 hours, heating slowly to burn out the binder. The parts shrink about 15% in each direction (more along the field in oriented parts); make the die that much bigger.
  8. Grind to size with silicon carbide or diamond. Ferrite is as hard and brittle as porcelain.
  9. Magnetise in a strong pulse field (below).

Bonded (rubber) magnets. Knead 85–90% by weight of fine ferrite powder into rubber (Rubber) or a plastic, roll it into sheet or strip, cure it, and magnetise it. It is weak but flexible and can be cut with scissors: door seals for refrigerators (Ice and Refrigeration), signs, toys.

Rare-earth magnets in outline

These are four to ten times stronger than alnico, by energy product. Making them is honest factory work, not workshop work.

  • Samarium–cobalt (SmCo₅). Needs samarium separated from the other rare earths by solvent extraction or ion exchange (Separating the Rare Earths). Samarium and cobalt are melted together under argon, ground to 3–5 µm grains under oil or nitrogen, aligned and pressed in a field of 1–2 T, sintered at 1,100–1,200 °C in argon or vacuum and heat-treated.
  • Neodymium–iron–boron (Nd₂Fe₁₄B). About 30% neodymium, 1% boron, the rest iron. Melted in vacuum, broken into powder by soaking up hydrogen, milled to 3–5 µm in nitrogen, aligned, pressed and sintered at about 1,050–1,100 °C in vacuum, then annealed. It rusts quickly and must be nickel-plated (Electroplating). Its powder catches fire in air.
  • A nearer goal: mischmetal–cobalt. Mischmetal (Rare Earths, Cerium and Phosphors) needs no separation. Alloyed with cobalt in the ratio of SmCo₅ and made the same way, it gives magnets well above alnico in strength, though well below true samarium–cobalt.

The magnetiser

NS Yoke magnetiser Soft-iron yoke Flux round the loop Coils Pole screws down Magnet no air gap battery bank, 10–30 A switch Pulse magnetiser Clamping frame coil tries to burst Coil 10–50 turns copper strip Magnet ferrite, rare-earth Heavy switch Bleed resistor empties the bank Capacitor bank 4,000–10,000 µF, 300–450 V, from a charger
Fig. 3 Two magnetisers. Left: a direct-current electromagnet with a soft-iron yoke; the magnet is clamped between adjustable pole pieces. Right: a pulse magnetiser; a capacitor bank or battery dumps a huge current for an instant through a few turns of heavy copper around the magnet.

Stroking (Magnets) is fine for compass needles but can only bring a magnet to a fraction of its strength. A magnet must be driven by a field three to five times its coercivity:

Material Field needed
Carbon, tungsten, chrome steel 25–50 kA/m
Cobalt steel about 100 kA/m
Alnico 250–300 kA/m
Ferrite 800–1,000 kA/m
Rare-earth 2,000–3,000 kA/m

The yoke magnetiser (for steel and alnico)

  1. Yoke. Forge or cast a C-shaped frame of soft iron (Iron (the Bloomery)) about 50 × 50 mm in section, with a gap that can be closed by two adjustable pole pieces — soft iron blocks on screws.
  2. Coils. Wind two coils on the yoke's arms, each about 500 turns of heavy insulated copper wire, 1.5–2 mm thick (Copper Wire), joined so both drive the field the same way round.
  3. Power. A lead-acid bank or dynamo giving 10–30 A (The Rechargeable Battery, The Generator).
  4. Use. Screw the pole pieces against the magnet's ends so there is no air gap. The field in the magnet is roughly ampere-turns ÷ magnet length: 1,000 turns at 20 A across a 5 cm magnet gives 400 kA/m — enough for alnico. Switch on for 1–2 seconds, switch off slowly through a resistance (a sudden break gives a dangerous high-voltage spark), and slide a keeper on before taking the magnet off the poles.

For a horseshoe, lay its pole faces flat on the two pole pieces instead.

The pulse magnetiser (for ferrite and rare-earth)

Iron saturates at about 2 T and cannot carry the field these need. Use an air coil and a very short, very large current instead:

  1. Coil. 10–50 turns of thick copper strip or bar, wound tightly around a former just big enough to take the magnet, clamped hard in a heavy wooden or bronze frame: the coil tries to burst outwards at every pulse.
  2. Energy. A bank of large capacitors (Resistors, Capacitors and Coils) — for example 4,000–10,000 µF charged to 300–450 V, storing 200–1,000 J. Or, without capacitors, short a large battery bank through the coil for a fraction of a second.
  3. Switch. A heavy mercury or thyristor switch (Power Electronics and Motor Drives), or a sturdy knife switch for battery pulses.
  4. Use. Put the magnet in the coil, oriented as wanted, stand back, close the switch. Peak currents are thousands of amperes for a few thousandths of a second; the coil bangs and warms.

Keepers and care

  • Steel and alnico magnets must always have a keeper — a bar of soft iron across their poles — when not in use, and must never be pulled apart from their pole pieces without one. Taking alnico out of its circuit can lose a third of its strength.
  • Ferrite and rare-earth magnets do not need keepers.
  • Stabilise magnets for meters and clocks by knocking them down 5–10% (a weak reverse pulse, or a few hours at 100 °C), so they will not drift later.
  • Do not drop, hammer, heat or store magnets touching others in a jumble.

How to tell it worked

  • Lift test. Hang a soft-iron keeper from a spring balance (Balances, Steelyards and Weighing Machines), put it on the poles, and pull. Compare with a known good magnet of the same size and shape.
  • Compass deflection. Put a compass on a table with the magnet laid east–west, its end a fixed distance (say 20 cm) from the needle. The stronger the magnet, the further the needle swings. Use the same distance and position every time.
  • Search coil. Wind 50 turns of thin wire into a loop that just slips over the magnet, connect it to a galvanometer (Measuring Electricity) and pull the loop off the magnet sharply. The size of the kick is proportional to the magnetism. Good for comparing a batch.
  • Iron filings sprinkled on paper over the magnet show where the poles are. Extra poles in the middle of a bar mean it was magnetised unevenly.
  • Ferrite grain. A broken ferrite magnet shows a dull, even, very fine grey grain, without visible crystals or cracks.

Note Troubleshooting. Steel magnet weak → not fully hardened (a file bites it), tempered, too short and thick, or magnetised by stroking only. Re-harden, and use a coil. Steel magnet loses strength in weeks → not aged, or stored without a keeper. Alnico 5 no better than alnico 2 → it cooled too fast or too slow, or without enough field, or across the wrong axis. Re-solution and repeat. Alnico cracks → mould too hard or cooling too fast after casting; use weaker sand and bury the castings in ash. Ferrite weak → grains too coarse (grind longer), fired too hot (grains grew), not oriented, or under-magnetised. Ferrite cracks or warps in the kiln → uneven pressing, binder burned off too fast, or kiln too hot at one side.

Dangers

Danger Stored electricity. A capacitor bank charged to a few hundred volts kills, and it stays charged after the power is off. Fit a bleed resistor across it, short it with an insulated bar before touching anything, and keep one hand in your pocket. Breaking the current of a large magnetiser suddenly gives a high-voltage spark; switch off through a resistance.

Danger Molten alnico at 1,600 °C, and aluminium added to it, throw out burning metal; any damp tool or mould makes it explode. Preheat every tool, wear face protection and leather, and see Metal Casting.

  • Barium compounds are poisonous if swallowed or breathed. See The Vacuum Tube. Wear a damp mask when handling ferrite powders.
  • Cobalt and nickel dusts harm the lungs and skin. Grind wet.
  • Strong magnets snap together with force enough to crush fingers and shatter ferrite or rare-earth magnets into sharp flying chips. They wreck watches and compasses, and they can stop a heart pacemaker. Slide magnets apart, do not prise them.
  • Rare-earth powders catch fire in air.

What this unlocks

Strong, small magnets make magnetos for engines, bicycle dynamos, and permanent-magnet motors and generators (The Electric Motor, The Generator, Wind Turbines, Electric Vehicles); moving-coil meters (Measuring Electricity, Electricity Meters and Billing); telephone receivers, microphones and loudspeakers (The Telephone, Loudspeakers, Microphones and Headphones); magnetrons for radar and ovens (Radar and Microwaves); magnetic separators for ore and grain (Mining and Tunnelling); and the magnetic chucks of grinding machines (Precision Grinding). Soft magnetic materials, the opposite job, are in Transformer Steel, Ferrite and Magnetic Shielding.

How it was first done

For centuries the only magnets were lodestones and steel stroked on them. Gowin Knight in London made unusually strong steel magnets in the 1740s by careful stroking of hardened steel bars. Hardened tungsten steel magnets came into use in the late 19th century. Kotaro Honda in Japan invented cobalt-rich KS steel in 1917. Tokushichi Mishima in Japan discovered the iron–nickel–aluminium MK steel in 1931, which led to alnico, improved in Britain, the USA and the Netherlands in the 1930s; cooling in a magnetic field was found around 1938. Philips in the Netherlands introduced barium ferrite magnets ("Ferroxdure") in 1952. Samarium–cobalt magnets were developed in the USA in the late 1960s, and neodymium–iron–boron in 1982–1984, independently by Masato Sagawa at Sumitomo in Japan and by General Motors in the USA.

Source: content/entries/metals/permanent-magnets.md