◆ Rebuild

Part 5 · Cloth and Clothing

Flax, Hemp and Linen

Grow flax or hemp, pull it, rot away the glue in water or dew, then break, scutch and comb the stems until only long, silky fibre is left — the raw material of linen, sailcloth, rope and the best paper. Nettle and other bast fibres work the same way.

Difficulty
●●●●●
Time
About 100 days to grow; 1–6 weeks to ret; a few days of hard work per 10 kg of stems to break, scutch and heckle
Steps from zero
3 prerequisites →

You need first

Farming from SeedCordage and Rope

This unlocks

Ropewalks and Sailcloth
The full path from nothing — 3 steps before this one
  1. Stone Tools
  2. Cordage and Rope
  3. Farming from Seed
  4. Flax, Hemp and Linen

Do them roughly in this order. See it on the tech tree →

Why it matters

Before cotton travelled the world, the cloth of Europe, Egypt and the Middle East was linen — cloth made from the stem fibres of the flax plant. Linen is strong, cool, washes well and gets stronger when wet. It made shirts, sheets, bandages (Wound Care and Antiseptics), sacks, sails, fishing nets and bowstrings. Worn-out linen rags were the raw material of Paper for a thousand years. Hemp, flax's taller, coarser cousin, made the world's ropes, sailcloth and canvas until the 20th century. The seed of flax (linseed) is pressed for a drying oil that becomes paint, varnish and printing Ink.

These plants matter for a simple reason: they grow almost anywhere with a temperate summer, they need no animals, and one season turns a small plot of land into kilograms of long, strong fibre. Once you can make fibre, you can spin it (Spinning and Weaving Cloth), weave it (The Loom), and sew it (Sewing, Needles and Thread) into everything from clothes (Making Clothes) to sails (Boats and Sails).

How it works

Flax, hemp and nettle are bast fibre plants. Their stems are built like a pipe:

Skinthin, papery; flakes off Fibre bundlesthe part you want: a ring of long cellulosestrands running the whole length of the stem Pectin glueholds fibre to skin and wood;retting rots it away Woody corebrittle when dry; breaks into "shives"(the hollow middle is soft pith) AFTER RETTING AND BREAKING shives fall away;fibre stays whole Flax stem, cut acrossreal size 1–3 mm thick (shown enlarged)
Fig. 1 A flax stem in cross-section. The useful fibre lies in bundles in a thin ring just under the skin, glued to its neighbours and to the woody core by pectin. Retting rots the glue; breaking and scutching knock the woody core away.
  • Skin (epidermis) on the outside, thin and papery.
  • Bast fibre bundles in a ring just inside the skin. Each fibre is a single long, thin cell, mostly 1–5 cm long, made of almost pure cellulose — the same stuff as cotton and paper. The cells overlap in bundles that run the full length of the stem.
  • Woody core inside, brittle when dry. Its broken pieces are called shives (or boon).

Everything is held together by a natural glue called pectin — the same substance that sets jam. You cannot simply peel good fibre off; it comes away stuck to skin and wood. The trick is retting (an old word for "rotting"): soak the stems or leave them in damp grass, and bacteria and fungi eat the pectin before they get round to the tougher cellulose. Stop at the right moment and the fibre falls free of the wood. Stop too early and it stays glued; leave it too long and the fibre itself rots and goes weak.

After retting, three mechanical steps clean the fibre:

  1. Breaking — crush the dry stems so the brittle woody core shatters into short pieces, while the flexible fibre bends and survives.
  2. Scutching — beat and scrape the broken stems with a wooden blade to knock out the shives.
  3. Heckling (also spelled hackling) — pull the fibre through combs of spikes, coarse then fine, to split the bundles into fine strands and to separate the long fibres (line) from the short, tangled ones (tow).

Line is spun into fine, smooth, strong thread. Tow is spun into coarser yarn for sacking, rope and rough cloth — nothing is wasted.

What you need

Item Amount or size Notes
Flax seed (fibre type) or hemp seed 10–15 g per m² for flax (about a heaped tablespoon); 5–8 g per m² for fibre hemp Sow thickly: crowded plants grow tall and unbranched, which is what you want
Land 100 m² (10 × 10 m) for a first crop Gives roughly 40–60 kg of dry stems and 4–8 kg of clean fibre — enough for several shirts
Retting place A pond, ditch or slow stream away from drinking water; or a meadow for dew retting See Dangers
Ripple comb A board with a row of wooden or iron teeth 15–20 cm long, 5 mm apart Strips seed heads off flax
Flax brake Hinged wooden jaws, about 1 m long See below; a mallet and a log will do at first
Scutching board and knife Upright board 1 m tall with a notch at the top; flat wooden "sword" 50–60 cm long
Heckles Two or three boards set with spikes: coarse (spikes 1.5–2 cm apart), medium (1 cm), fine (5 mm) Iron nails are best; hardwood or bone pegs, or blackthorn spines, will do

The brake, scutching knife and heckles are simple Basic Woodworking. Iron spikes for heckles come from Nails, Rivets and Wire Fasteners or Blacksmithing.

1. BREAK Flax brakehinged jaws about 1 m long;slam the top jaw down ondry stems laid across stemsend view: blades crush the coreinto a zigzag, fibre bends 2. SCUTCH Board and knifeboard 1 m tall, notched;wooden knife 50–60 cmKnife scrape down the hanging fibre shivesfly off 3. HECKLE Comb of spikescoarse, then medium, then fine;pull each handful through Linelong, silky — fine thread Towshort, tangled
Fig. 2 The fibre tools. The brake crushes the dry stems; the scutching knife scrapes the broken shives out; the heckle combs the fibre into long "line" and short "tow".

Where to find it

  • Flax (Linum usitatissimum) is a slender annual 60–120 cm tall with narrow grey-green leaves and small sky-blue (sometimes white) five-petalled flowers that open in the morning and drop by afternoon. The round seed heads ("bolls") hold up to ten flat, shiny brown seeds. Seed survives in old seed stores, in bags of linseed sold as food or animal feed, and wild flax relatives grow on dry grassland in Europe and Asia — though wild flax has shorter fibres and seeds that shatter. Seed bred for oil gives short, branched plants with poor fibre; seed of fibre flax gives tall single stems. Grow what you can find and save seed from your tallest plants (Saving Seed and Breeding Plants).
  • Hemp (Cannabis sativa) grows 1–4 m tall, with leaves split like a hand into 5–9 narrow, saw-edged leaflets and a strong resinous smell. It escapes from cultivation and grows on disturbed, fertile ground, river banks and old field edges. Male and female flowers usually grow on separate plants; the males (with dangling flower clusters) ripen and die a few weeks before the females (with tight leafy heads that make seed).
  • Stinging nettle (Urtica dioica) grows in dense patches on rich, damp ground near streams and old settlements. Square stems, opposite toothed leaves, stinging hairs. Tall stems cut in late summer or autumn give a fine, silky fibre that was woven into cloth in Europe for thousands of years. See Cordage and Rope for identification.
  • Other bast fibres — ramie (China grass, a non-stinging nettle relative of warm Asia, with leaves silvery-white underneath) gives the longest and most lustrous plant fibre; jute (warm, wet lowlands of South Asia) gives coarse sacking fibre; the inner bark of lime/basswood and willow gives coarse cord and matting. All are retted and cleaned in the same way.

Step by step: flax to linen fibre

1. Grow it

  1. Choose ground. Fertile, well-drained, weed-free soil that held a different crop last year. Flax hates weeds (it cannot shade them out) and hates waterlogging. Do not grow flax on the same land more than once in six years: soil diseases build up. See Farming from Seed.
  2. Sow in spring as soon as hard frosts end — in temperate lands about when the oak and birch leaf out. Make a fine, firm seedbed, scatter the seed evenly at 10–15 g per m², rake it in about 1–2 cm deep, and firm it with a board or roller. The plants should come up so close that they nearly touch: about 1,500–2,000 stems per square metre.
  3. Weed once, carefully, when the seedlings are a hand high (10 cm). After that they close over the ground.
  4. Watch them grow. Flax needs about 90–110 days. It flowers about 50–60 days after sowing, for two to three weeks.

Hemp is sown the same way, a little later (when the soil is warm to the hand), at 5–8 g per m². It shoots up fast — up to 5 cm a day in midsummer — and smothers weeds by itself.

2. Pull it

  • When: for fibre and seed, when the lower third of the stems has turned yellow and lost its leaves, and the seed bolls are turning from green to brown. Pulled earlier, while still green and flowering, flax gives the finest, softest fibre but no seed. Left later, until the stems are fully brown, the fibre is coarse and brittle.
  • How: grip a handful of stems just below the seed heads and pull them up by the roots. Do not cut. Pulling keeps the full length of fibre (which runs right down into the root), and cut ends let water and rot into the stems unevenly during retting. Knock off the soil and lay the handfuls with all the roots at one end.
  • Ripple off the seed. Drag the seed heads through the teeth of the ripple comb. Dry the seed heads in the sun, thresh them, and keep the best seed for next year; press the rest for linseed oil (Oils and Pressing).
  • Hemp is cut close to the ground with a sickle (Sickle, Scythe and Hand Harvest Tools) because its stems are too strong to pull. Cut the males when their flowers have shed pollen and the stems start to yellow; the females a few weeks later if you want seed.

3. Ret it

Water retting is faster and gives a paler, more even fibre:

  1. Tie the stems in bundles as thick as your thigh, all roots one way.
  2. Sink them in still or slow water — a pond, a pit lined with clay, a ditch — weighted with stones or logs so they stay under. Soft water (rain or river water) works better than hard spring water.
  3. Wait. In water at 20–30 °C (pleasant to swim in) retting takes 5–10 days; in cold water it can take 2–3 weeks. Bubbles rise and the water turns brown and smells strongly of rotten cabbage.
  4. Test daily from day 4. Pull out a few stems, let them dry a little, and bend them. When the woody core snaps cleanly and the fibre peels away from it along the whole length, without sticky green strands holding on, the retting is done. Fibre that still clings to the wood: wait a day. Fibre that breaks when you tug it: you are late — take the rest out at once.
  5. Lift the bundles out, rinse them in clean water, and stand them in loose cones ("stooks") in the sun and wind to dry completely, for a week or more.

Dew retting needs no pond and is gentler, but slower:

  1. Spread the pulled stems thinly on short grass, a single layer, all one way.
  2. Leave them 2–6 weeks, turning them over with a long pole every week so both sides ret evenly. Dew, rain and the fungi in the grass do the work. Late summer, with warm days and heavy dews, is best.
  3. The stems turn from yellow to silver-grey. Test them in the same way as water retting.

Nettles are retted the same way; in water they take about 1–2 weeks. Hemp takes about as long as flax, sometimes a little longer.

4. Dry it thoroughly

Breaking works only on bone-dry stems: the woody core must snap, not bend. Store retted stems under a roof. Just before breaking, dry them again in the sun on a hot day, or on a rack near (never over) a fire or in a warm, empty bread oven. Many flax-house fires started this way — see Dangers.

5. Break it

The flax brake is two hinged wooden jaws. The lower jaw is a heavy beam with two or three parallel blades (thin vertical boards, edges rounded, not sharp) about 2–3 cm apart; the upper jaw has one or two blades that fit down between them. Each blade is about 1 m long. The upper jaw is hinged at the far end and has a handle at the near end.

  1. Lay a handful of stems across the lower jaw.
  2. Bring the upper jaw down hard, again and again, feeding the stems slowly through and moving along their length. You hear the woody core crack.
  3. Turn the handful round and break the other end.

Without a brake, lay the stems on a flat log and beat them with a wooden mallet or a flat-sided club along their length.

6. Scutch it

The scutching board is an upright board about 1 m tall fixed to a heavy base, with a notch cut in the top edge. The scutching knife is a flat, wooden blade like a sword, 50–60 cm long, 10 cm wide, with thin but not sharp edges.

  1. Hold a small handful of broken flax by one end and hang the other half over the notch so it lies against the face of the board.
  2. Strike down along the face of the board with the knife, glancing blows that scrape downwards along the fibre. The shives fly off.
  3. Turn and shift the handful often. When one half is clean and soft, turn it round and scutch the other half.

Scutching is hard, dusty work. Work outdoors, and stop when what is left is a soft, golden or silvery hank with only occasional bits of wood. The short fibres knocked off are coarse tow — save them for stuffing, caulking and rough cord.

7. Heckle it

A heckle (hackle) is a board with a bed of upright spikes, fixed to a bench.

  1. Start on the coarse heckle. Wrap the top of a handful of scutched fibre once round your hand. Throw the free end onto the spikes, near the tips at first, and pull it through towards you. Then a little deeper. Then all the way.
  2. Comb the free half until it slides through without catching, then turn the handful round and do the other half.
  3. Move to the medium heckle, then the fine one.
  4. What stays in your hand is line: long, smooth, shiny fibre, often 50–90 cm long. What stays caught on the spikes is tow: short, tangled fibre.

Twist each handful of line loosely into a "strick" (a soft hank folded on itself) and store it dry. Line is ready to dress on a distaff and spin (Spinning and Weaving Cloth). Tow is carded like wool (Wool) and spun into coarser yarn. Expect a total fibre weight of roughly one tenth to one sixth of the dry stem weight, of which perhaps half or more is line.

Linen and its properties

Linen thread is spun from line, usually with the fibre kept damp (spinners wet their fingers or keep a little bowl of water at hand), which makes a smoother, stronger yarn. Linen cloth is:

  • Strong — clearly stronger than cotton, and stronger still (by roughly a fifth) when wet. It lasts for generations.
  • Cool and absorbent — it takes up moisture and dries fast, which makes it the best summer cloth and the best for towels and bandages.
  • Stiff and unstretchy — it hardly gives at all, so it keeps its shape in sails and sacks, but it creases badly and is less warm than wool.
  • Easy to clean — it can be boiled, and it takes washing with Soap and weak Lye and Potash. New linen is grey-brown; repeated washing and laying it out on grass in the sun bleaches it slowly to white (Laundry and Bleaching Cloth, Chlorine and Bleach).
  • Hard to dye in deep colours compared with wool — see Dyes and Mordants.

Hemp cloth is coarser, heavier and even stronger; it was the canvas of sails, tents, sacks and work clothes. Hemp fibre is also the best plant fibre for rope (Cordage and Rope). Nettle cloth is finer than hemp and feels like a soft linen.

How to tell it worked

  • Good retting: the dry stem snaps cleanly and the fibre strips off along its whole length in one go, leaving a bare white woody core.
  • Good line: long (more than half the length of the stem), soft, smooth, with a silky shine, golden-grey to silver. It rustles, and pulling hard on a pencil-thick strand between your hands should not break it.
  • Clean enough: you can see no more than a few flakes of shive per handful. Shives make spinning lumpy.

Note Troubleshooting. Fibre stays glued to the wood → under-retted. Put it back in the water or on the grass. If it is already dry, re-wet and ret it again. Fibre is weak and breaks when you heckle → over-retted, or it went mouldy while drying. Next time test more often and dry quicker. The core bends instead of snapping in the brake → the stems are damp. Dry them in hot sun or a warm oven for an afternoon. Most of the fibre ends up as tow → you heckled too hard at the start (begin with the tips), the stems were too short or branched (sow thicker, use fibre seed), or they were pulled too late. Fibre is patchy brown → stems were not turned during dew retting, or the bundles were too tight in the water.

Dangers

Danger Flax and hemp dust burns explosively. Dry stems, shives and fibre dust catch fire from one spark, and a cloud of fine dust in a closed room can flash into flame. Dry the stems in the sun or well away from open flame — never on a rack directly over a fire. Keep scutching sheds clean and keep fire out of them.

  • Dust in the lungs. Breathing flax and hemp dust day after day causes a chronic cough and tight chest. Break and scutch outdoors, with your back to the wind, and tie a damp cloth over nose and mouth.
  • Retting pollutes water. A retting pond uses up the oxygen in the water and fills it with rotting matter; it kills fish and makes the water unsafe to drink. Many old laws forbade retting in rivers. Use a pond or pit set aside for it, well downstream of any drinking supply (Finding and Purifying Water, Sanitation and Germs).
  • Hemp flowers of some varieties contain a drug that affects the mind. Fibre varieties contain little of it. Grow hemp for its stems and seed.
  • Nettle stings are painful but harmless; wear leather gloves or wrap your hands in leaves.
  • Linseed oil rags can heat up and burst into flame by themselves as the oil dries. Spread them flat outdoors to dry or keep them in water. See Oils and Pressing.

What this unlocks

Linen thread and cloth: Spinning and Weaving Cloth, The Loom, Sewing, Needles and Thread, Making Clothes. Sailcloth and rope: Boats and Sails, Cordage and Rope. Rag fibre for Paper. Clean dressings for Wound Care and Antiseptics. Linseed oil for Ink and Pigments, Paints and Varnish (Oils and Pressing). Linen tape, thread and cloth insulate wire (Copper Wire) and make strong fire hoses and drive bands (Belts, Chains and Power Transmission). The long-fibre line can also be cottonised — cut short and spun like Cotton — on Textile Machinery.

How it was first done

The oldest known flax fibres — some twisted, some apparently dyed — were found in Dzudzuana Cave in Georgia, in layers about 30,000 years old; the people there probably gathered wild flax. Flax was among the very first crops of the Fertile Crescent, about 9,000–10,000 years ago, and fragments of linen survive from Neolithic villages such as Çatalhöyük in Turkey and the lake dwellings of Switzerland. Ancient Egypt was the great linen land: mummies were wrapped in hundreds of square metres of it, and the finest Egyptian linen was almost transparent. Hemp was grown in China at least 5,000 years ago for cord and cloth. A cloth of nettle fibre wrapped the bones in a Bronze Age burial at Voldtofte in Denmark, about 2,800 years old. Until the cotton mills of the 1800s, most of Europe's shirts, sheets and sails were linen and hemp, prepared by hand exactly as this chapter describes.

Source: content/entries/textiles/flax-and-hemp.md