◆ Rebuild

Part 8 · Chemistry

Water Glass (Sodium Silicate)

Melt sand with soda or potash and you get a glass that dissolves in boiling water. Boiled down to a clear syrup, this "water glass" glues paper and pottery, keeps eggs fresh for months, makes wood resist fire, hardens floors and furnace cements, binds welding-rod coatings and foundry cores, and turns into silica gel for keeping things dry.

Difficulty
●●●●●
Time
Half a day to melt a batch; a day to dissolve and boil it down
Steps from zero
13 prerequisites →

You need first

Soda Ash and Baking SodaThe Kiln

This unlocks

—

Objects made here

water glass potsilica gel
The full path from nothing — 13 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. Sulfur
  4. Pottery
  5. The Kiln
  6. Charcoal
  7. Lime
  8. Salt
  9. Lye and Potash
  10. Glass
  11. Saltpeter
  12. Sulfuric Acid
  13. Soda Ash and Baking Soda
  14. Water Glass (Sodium Silicate)

Do them roughly in this order. See it on the tech tree →

Why it matters

Ordinary glass is made of sand, an alkali (soda or potash) and lime. Leave out the lime and use extra alkali, and the glass you get dissolves in hot water — a fact that annoyed glassmakers for centuries (Glass). Dissolved, it is a thick, clear, slightly greenish syrup: water glass, or sodium silicate.

That syrup turns out to be one of the handiest materials in a workshop:

  • Glue for paper, cardboard, labels on glass, mending pottery and sticking glass to glass.
  • Egg preserving: eggs laid in spring, kept in diluted water glass in a cool cellar, are still good to eat in winter (Preserving Food, Poultry and Eggs).
  • Fireproofing: painted on wood, cloth and paper, it makes them much harder to set alight.
  • Cements: mixed with fireclay or ground brick it is a heat-proof cement for stoves, furnaces and kilns (Firebrick and Refractories, Chimneys, Stoves and Heating); with lime-rich concrete and plaster it seals and hardens the surface.
  • Binder: it holds the coating on welding rods (Welding) and, hardened with carbon dioxide, binds sand into foundry cores (Metal Casting).
  • Silica gel: water glass and acid make a glassy jelly that dries to grains which suck moisture out of the air — for keeping seeds, medicines and instruments dry.

All from sand and the soda you already know how to make.

How it works

Sand is silica (silicon dioxide), the stuff of quartz. Heated with an alkali such as soda (sodium carbonate, Soda Ash and Baking Soda), the two react: carbon dioxide bubbles off and the rest melts into a glass of sodium silicate:

silica + soda → sodium silicate (glass) + carbon dioxide

The ratio of silica to alkali decides everything:

Sand : soda ash, by weight Silica-to-soda ratio Behaviour
1 : 1 about 1.8 Dissolves easily in boiling water. Strongly alkaline. Best first batch; good for eggs, cements, welding rods.
1.5 : 1 about 2.6 Dissolves slowly (a day of boiling, fine powder). A stronger, more water-resistant glue and binder.
2 : 1 about 3.5 Hardly dissolves without steam under pressure. Avoid.
Ordinary glass (with lime) — Does not dissolve at all.

The syrup sets in two ways. As it dries, it turns into a hard, clear glassy film. And acids — even the weak carbonic acid from carbon dioxide in the air — pull the soda away, leaving a gel of pure silica that slowly hardens. So water glass in an open pot grows a skin, and joints made with it keep getting harder for weeks.

1 Weigh and mix equal weights of dry sandand dry soda ash 2 Melt 1,100–1,250 °C until bubbling stops 3 Quench thin stream into cold water: frit 4 Grind and boil powder + 3–4× its weight of water; boil 4–8 hours 5 Boil down to syrup like thin honey: 1 litre weighs 1.35–1.4 kg 6 Test it dries to a clear film + acid: white jelly
Fig. 1 Making water glass. Sand and soda ash are mixed by weight, melted in a crucible until the bubbling stops, quenched in water so the glass shatters, then ground and boiled until it dissolves. Boiled down, the solution becomes the syrup.

What you need

Item Amount Notes
Clean sand or crushed quartz 2 kg White, fine, washed free of clay. See Glass.
Soda ash (sodium carbonate) 2 kg Dry. From Soda Ash and Baking Soda. Natron works if it is fairly pure.
or potash 2 kg Gives potassium water glass, which dissolves even more easily but stays slightly sticky (Lye and Potash).
Fireclay crucible 3–5 litres It must hold twice the volume of the batch, because the melt froths (Firebrick and Refractories).
Furnace 1 A glass furnace or a kiln with forced draught that reaches 1,100–1,250 °C — bright yellow-orange (Glass, The Kiln, Bellows).
Large iron pot or tub of cold water 30 litres For quenching the melt
Iron pot for boiling 15–20 litres Water glass eats aluminium and zinc. Iron, stoneware and glass are fine.
Mortar, sieve, wooden paddle, long iron tongs, leather gloves, eye protection

Where to find it

  • Sand and quartz: beaches, riverbeds and dunes; white quartz veins and pebbles, which you heat red-hot and drop into water so they crackle into crushable pieces (Glass). The whiter, the better; iron in the sand makes the glass green, which does no harm.
  • Soda: made from salt or plant ash (Soda Ash and Baking Soda), or collected as natron on the shores of desert soda lakes.
  • Rice husk (for Method 2): the papery husks left from milling rice. Burned slowly in a heap to a white or pale grey ash, it is about nine-tenths silica in a form that dissolves easily in lye. Black ash means it is not fully burned; burn it longer.
  • Diatomaceous earth (for Method 2): a very light, chalky white or pale grey rock or soil from old lake beds, made of the glassy shells of microscopic water plants. It feels like flour, does not fizz with acid (chalk does), and a lump floats briefly on water.

Method 1: Melting sand and soda

  1. Weigh and mix. Mix equal weights of dry sand and dry soda ash thoroughly — say 2 kg of each. Everything must be dry: damp batch spits in the furnace.
  2. Heat the crucible empty in the furnace to bright orange first.
  3. Charge it in portions. Shovel in about a third of the batch. It froths as carbon dioxide escapes. When the froth has died down, add the next third, and so on. Never fill more than half full.
  4. Melt. Keep the furnace at bright yellow-orange (1,100–1,250 °C) for 2–4 hours after the last charge, until the melt is clear and runny and no more bubbles rise when you lift some on an iron rod. A drawn thread should be glassy and free of white grains (undissolved sand).
  5. Quench. With tongs, pour the melt in a thin stream into the tub of cold water, standing well back and to the side. It shatters into small glassy lumps and crumbs (frit). Quenching makes it much easier to grind and dissolve. Alternatively pour it onto a dry iron plate and break it up when cold.
  6. Grind the frit to a fine powder, under 1 mm — like coarse flour. Wet-grind if you can, to keep down the dust.
  7. Dissolve. Put the powder in the iron pot with 3–4 times its weight of water and boil for 4–8 hours, stirring often and topping up water as it boils away. Most of it dissolves; a little grit settles.
  8. Settle and decant. Let it stand overnight. Pour or siphon off the clear liquid.
  9. Boil it down to a syrup like thin honey. Stop when a litre of it weighs about 1.35–1.4 kg (Measurement from Scratch) — roughly 35–40% solids, the strength used in this chapter. Thicker syrup gels in the pot.
  10. Store in glass, stoneware or iron with a tight lid. Open to the air it skins over. Glass stoppers stick fast in water glass; use a cork or a waxed wooden plug.

Tip Using saltcake. If you have saltcake (sodium sulfate, the by-product of making Hydrochloric Acid) instead of soda, melt it with sand and a little powdered charcoal. The charcoal helps break up the sulfate. Expect sulfur fumes; do it only in a furnace with a good chimney.

Method 2: Boiling silica in lye

If you have no furnace hot enough, you can dissolve a soft, non-crystalline silica in strong caustic soda. Ordinary quartz sand will not dissolve this way in useful time.

  1. Make caustic soda solution from soda ash and slaked lime (Soda Ash and Baking Soda, Lye and Potash).
  2. For each 1 kg of caustic soda (dry weight), take about 1.5 kg of white rice-husk ash or diatomaceous earth, and 4–5 litres of water.
  3. Boil them together in an iron pot for 2–4 hours, stirring. The silica dissolves; dirt and unburned carbon settle.
  4. Let it settle, filter through cloth, and boil down to syrup as in Method 1.

How to use it

Eggs under water glass 1 part syrup : 9 parts boiled water 5 cmof liquidabove eggs fresh, unwashed eggs, small end down; cellar below 15 °C; keep 6–9 months Fireproofing2–3 thin coats,last with chalk Furnace cement1 syrup : 3–4 fireclayor ground brick Silica gelwash, then bake120–150 °C diluted syrup into dilute acid → jelly
Fig. 2 Some uses of water glass. Eggs keep for months under diluted water glass in a cool cellar. Brushed on wood it slows fire. With fireclay it becomes a heat-proof cement. Poured into acid it sets to a jelly that dries to silica gel.

Preserving eggs

  1. Use fresh, clean, uncracked eggs, ideally less than two days old. Do not wash them: washing removes the natural coating that seals the shell. Wipe off dirt with a dry cloth.
  2. Mix 1 part water glass syrup with 9 parts boiled and cooled water.
  3. Stand the eggs, small end down, in a clean crock or wooden tub, and pour the liquid over them until they are covered by 5 cm. You can add eggs over several weeks as hens lay.
  4. Cover against dust and evaporation and keep in the coolest place you have — a cellar or a pit, ideally below 15 °C.
  5. They keep 6–9 months. Rinse before use. Before boiling them, prick the blunt end with a pin: the sealed shell otherwise cracks. Crack each egg into a cup first; throw away any that smells.

Glue

Brush thin syrup on both surfaces and press together. Paper and card stick in minutes; pottery and glass need a day. Joints are hard and heat-proof but softened by water at first. Warm them gently or brush on vinegar or dilute acid to make them more water-resistant. Not for food vessels.

Fireproofing wood and cloth

  • Wood: brush on 2–3 coats of 1 part syrup to 2–3 parts water, letting each dry; for the last coat stir in chalk or fine clay to make a paint. The film swells into a crust when heated and slows ignition from sparks and small flames. It will not stop a big fire, and rain washes it off outdoors.
  • Cloth and paper: dip in 1 part syrup to 4 parts water and dry. It stiffens the cloth and washes out in the laundry, so it suits curtains, theatre scenery and paper, not clothes.

Heat-proof cement

Stir 1 part syrup with 3–4 parts fireclay, grog or finely ground brick to a stiff paste (Firebrick and Refractories). Use it to bed firebricks, seal stove-pipes and patch cracks in kilns and furnaces (Chimneys, Stoves and Heating). Let it dry for a day, then heat it gently: it sets hard as stone. Mixed with fine quartz flour, a similar cement resists acids — useful for lining acid tanks (Sulfuric Acid).

Hardening concrete, lime and plaster

On a dry concrete or lime floor or wall, brush 2–3 coats of syrup diluted with 3–4 parts water, a day apart. It reacts with the lime to fill the pores, stops dusting and makes the surface harder and easier to wash (Mortar and Concrete, Portland Cement).

Binder for welding rods and foundry cores

  • Welding rods: see Welding, where water glass binds the flux coating.
  • Sand cores: mix clean, dry moulding sand with 3–5% of water glass by weight, ram it into the core box, and either bake it at 150–200 °C or blow carbon dioxide through it for a minute (from limestone and acid — Hydrogen, Oxygen and Gases). It sets hard at once (Metal Casting).

Silica gel

  1. Mix 1 part syrup with 3 parts water.
  2. Pour it slowly, stirring, into dilute acid (Sulfuric Acid or Hydrochloric Acid, 1 part acid in 10 parts water) until a drop of the mix just turns red-cabbage juice pink (Acids, Bases and Testing).
  3. In minutes to hours, the liquid sets to a clear jelly. Break it up and wash it many times in clean water over two or three days, to remove the salt.
  4. Dry it slowly, then bake at 120–150 °C (hot enough to brown paper slowly) for a few hours. It becomes hard, glassy grains.
  5. In a closed jar the grains keep seeds, instruments, medicines and iron tools dry. When they stop working, bake them again.

How to tell it worked

  • The glass dissolves almost completely in boiling water. Ordinary glass does not.
  • The syrup is clear to slightly green, slippery like soap between the fingers (wash at once), turns red-cabbage juice green (alkaline), and dries on a glass plate to a clear, hard, glossy film.
  • The acid test: a few drops of vinegar or acid stirred into a spoonful of syrup turn it into a white jelly. Sugar syrup or gum does not do this.
  • Eggs: after three months, a test egg cracked into a cup has a firm yolk and no bad smell.

Note Troubleshooting. Melt full of white grains → not hot enough or not long enough, or too much sand. Hotter, longer; or 1 : 1. Glass will not dissolve → too much sand, too coarse a powder, or lime in the batch (did you use shells or chalky sand?). Grind finer; next time add more soda and use lime-free sand. Syrup turns to jelly in the pot → boiled down too far, or acid fumes got into it. Add hot water and stir. Syrup cloudy → fine silt; let it settle longer and decant. Glue joints fail in damp → normal for fresh water glass; use the 1.5 : 1 glass, or harden the joint with acid or heat. Eggs taste strange or the whites run → eggs were not fresh or the store was warm.

Dangers

Danger Molten glass and water. Pouring the melt into water makes it burst and spit; a wet or cold crucible or tongs can make a steam explosion that throws molten glass. Pour in a thin stream, from the side, into plenty of water, wearing leather gloves, apron, boots and eye protection. Keep everyone else back. See also the dangers in Glass.

  • Water glass is alkaline, like weak Lye and Potash. In the eyes it can cause serious burns: rinse at once with plenty of clean water for 15 minutes. On skin it dries tight and cracks it; wash it off.
  • Silica dust from grinding sand, quartz, frit or dry silica gel causes silicosis, a crippling lung disease, over years. Grind wet, work in the open, and cover your mouth and nose with damp cloth.
  • Caustic soda in Method 2 burns badly; see Lye and Potash.
  • Hot syrup spits as it thickens; stir it, and keep your face out of the way.

What this unlocks

Months of stored eggs; cheap glue for packaging and Bookbinding; fire-resistant theatres, granaries and roofs (Firefighting); harder floors and better furnaces; sand cores for casting engine cylinders (The Internal Combustion Engine); welding rods; silica gel to keep stores and instruments dry; and, with acid, the pure silica that is one step towards Pure Silicon and silicon chemistry (Silicones and Synthetic Rubbers). Water glass is also a filler in Soap and a softener for laundry water (Laundry and Bleaching Cloth).

How it was first done

Alchemists of the 1600s knew that sand melted with plenty of alkali gave a glass that dissolved in water: Jan Baptist van Helmont described it around 1640, and Johann Rudolf Glauber made a "liquor of flints" in 1648. It stayed a curiosity until the Bavarian mineralogist Johann Nepomuk von Fuchs in Munich worked out how to make it reliably around 1818, described it in 1825, and proposed it to fireproof the woodwork and scenery of Munich's theatre after the fire of 1823. In the 1840s–1850s the French chemist Frédéric Kuhlmann used it to harden stone and plaster, and in 1878 Adolf Keim patented the silicate wall paints still used today. In the late 1800s and early 1900s "water-glassing" eggs became a common way to store them, especially during the two World Wars. After the Second World War, foundries began hardening water-glass sand cores with carbon dioxide.

Source: content/entries/chemistry/water-glass.md