Nothing — start here.Why it matters
An ore is a rock that contains enough of a metal, in a form you can get out, to be worth the work. Metal does not lie around in bars. Apart from a little native copper, gold and the odd iron meteorite, every knife, nail, wire and pot in the world began as a coloured or unusually heavy rock that somebody recognised.
Learning to read the ground is therefore the gate to the whole metals part of this book: Copper Smelting and Bronze for the first metal tools, Lead for pipes and solder, and Iron (the Bloomery) — which, once you can find it, is almost everywhere. Later, ores also give you Magnets (from magnetite), pigments and Dyes and Mordants (ochre, malachite), and Sulfur (from roasting sulfides).
You do not need to be a geologist (though Rocks and Minerals helps). You need to know about a dozen minerals well, a handful of places to look, and five simple tests.
How it works
Metals are reactive. Over millions of years most of them combine with oxygen, sulfur or carbon dioxide and become minerals — natural compounds that look nothing like metal: green, blue, red, black or brassy crystals. Smelting (see Copper Smelting and Iron (the Bloomery)) is simply the reverse: heat and carbon tear the oxygen back off.
Ore minerals get concentrated in four main ways, and each one tells you where to look:
- Veins. Hot water deep underground dissolves metals and deposits them in cracks as it cools. The cracks fill with white quartz (glassy, too hard to scratch with steel) or calcite (soft, fizzes in acid), with ore minerals scattered through. Veins show at the surface as pale stripes cutting across the rock, often along valleys and fault lines.
- Weathering caps (gossans). Where a sulfide vein reaches the surface, rain and air rot it. Iron stays behind as rusty, spongy rock — the gossan or "iron hat" — while copper moves a little and is re-deposited as green malachite and blue azurite just below. A rusty, cavernous outcrop with green stains is the classic sign of copper.
- Placers. Rivers wear rock down and sort the pieces by weight. Heavy minerals — cassiterite, magnetite, gold — drop out where the water slows: inside bends, behind boulders, in cracks of the bedrock. Black sands on beaches are the same thing, sorted by waves.
- Bog and lake ores. Groundwater picks up dissolved iron from sandy soils; where it seeps into a bog and meets air, the iron settles out as rusty bog iron. A bog that has been cut can grow a new crop in 20–30 years.
What you need
| Item | Use | How to make it |
|---|---|---|
| Streak plate | Rub a mineral on it to see the colour of its powder | The unglazed bottom of a fired pot, or any broken piece of fired clay (see Pottery). A rough flat stone of white quartzite also works. |
| Hammerstone | Break rocks to see fresh, unweathered faces | A fist-sized, tough, rounded river cobble (see Stone Tools). |
| Lodestone or magnet | Find magnetic iron minerals | A piece of magnetite that attracts iron grains, hung on a thread. Later, magnetised iron (see Magnets). |
| Scratch tools | Test hardness | Your fingernail, a copper bead, a steel knife if you have one, and a piece of quartz. |
| Pan | Concentrate heavy minerals from sand | A wide shallow wooden bowl (see Basic Woodworking) or a clay dish 30–40 cm across with sloping sides. |
| Bags or baskets | Carry samples | Leather pouches or Baskets and Containers. Label each sample with where you found it. |
Where to find it
Read the landscape first, then the rocks.
- Look at stream beds before hillsides. A river is a free sampling machine: it brings you pebbles from everything upstream. Walk up a stream checking the gravel. When a type of pebble (green-stained, heavy black, rusty) stops appearing, its source is somewhere just above, often in a side valley.
- Look for colour. Green and blue stains mean copper. Rust red, orange and yellow mean iron (and sometimes a gossan over other metals). Bare patches where plants grow poorly can mean metal-rich soil.
- Look for old workings. In a ruined world, old mines, spoil heaps and slag piles are gold mines of ore and leftover metal. Tip heaps contain the minerals that were dug out alongside the ore — study them.
- Copper — in hilly or mountain country with dark volcanic rocks, in deserts (where green stains survive well), in old basalt flows (native copper), and under gossans.
- Tin — almost always near granite (a coarse, speckled rock of white, pink and black grains). Pan the streams that drain granite moors and hills.
- Lead — in veins in limestone country, often with calcite, fluorite (glassy purple, green or yellow cubes) and zinc ore.
- Iron — practically everywhere: red soils and rocks, bogs, black beach sand, ironstone nodules in shales near coal.
The five field tests
Always test a fresh surface. Weathered outsides are stained and misleading; break the rock open with your hammerstone.
- Colour and shine. Is the fresh break metallic (shines like metal), glassy, or dull and earthy? Note the colour, but do not trust it alone — one mineral can come in many colours.
- Streak. Rub the mineral firmly across your unglazed pottery. The colour of the powder line is very reliable. Hematite always gives cherry-red to red-brown even when the rock is black; magnetite gives black; bog iron gives yellow-brown; malachite pale green. Brassy minerals give greenish-black.
- Weight (heft). Ordinary rock (quartz, granite, sandstone, limestone) weighs about 2.6–2.7 times as much as the same volume of water. Most ores are much heavier: iron oxides about 5 times, cassiterite about 7, galena 7.5, native copper 9. Pick up a fist-sized ordinary pebble in one hand and the sample in the other. Ore feels "wrong" — unexpectedly heavy, like it is made of metal.
- Magnetism. Hang your lodestone on a thread and bring the sample close, or put crushed sample grains near it. Magnetite jumps. Most other iron ores do not, until roasted with a little charcoal (see below), when they turn black and magnetic — this is a quick way to confirm any iron ore.
- Fire tests. Crush a pinch of the mineral and sprinkle it on glowing coals:
- A green or blue-green flame means copper.
- A smell of burnt matches or rotten eggs means a sulfide (sulfur).
- A garlic smell and white smoke means arsenic. Step back upwind at once (see Dangers).
- Bright lead beads sweating out of a grey mineral on charcoal mean galena.
Hardness helps too. A fingernail scratches minerals up to about 2.5; copper scratches up to about 3; a steel knife or glass about 5.5; quartz about 7. If a mineral scratches glass, it is hard (cassiterite, quartz); if it can be scratched by copper, it is soft (galena, malachite).
The key ores
| Ore | Metal (pure mineral) | Looks like | Streak | Heft | Other tests |
|---|---|---|---|---|---|
| Native copper | Copper, ~100% | Brown-black lumps, green crust; pink metal when scratched | Shiny copper | Very heavy | Bends and flattens under a hammer |
| Malachite | Copper, 57% | Bright green, banded like an onion | Pale green | Moderate (4) | Green flame; fizzes in hot vinegar |
| Azurite | Copper, 55% | Deep blue crusts and crystals | Light blue | Moderate (3.8) | Green flame; found with malachite |
| Chalcopyrite | Copper, 35% (+ iron) | Brassy yellow, often rainbow-tarnished | Greenish black | Moderate (4.2) | Knife scratches it; sulfur smell when heated |
| Cassiterite (tin) | Tin, 79% | Brown-black glassy grains and pebbles | White to pale brown | Very heavy (7) | Too hard for a knife; stays in the pan |
| Galena (lead) | Lead, 87% | Bright lead-grey cubes | Grey-black | Extremely heavy (7.5) | Breaks into perfect cubes; soft |
| Hematite (iron) | Iron, 70% | Steel-grey, black or earthy red | Cherry red | Heavy (5.3) | Magnetic only after roasting with charcoal |
| Magnetite (iron) | Iron, 72% | Black, heavy | Black | Heavy (5.2) | Strongly magnetic |
| Bog iron / limonite | Iron, 40–60% as found | Rusty brown porous lumps and crusts | Yellow-brown | Moderate (3.5–4) | Turns red, then black and magnetic when roasted |
| Siderite (iron) | Iron, 48% | Tan to brown, curved crystal faces | White to pale tan | Moderate (3.9) | Fizzes in warm acid; darkens and turns magnetic when roasted |
Warning Look-alikes. Pyrite ("fool's gold") is paler and harder than chalcopyrite — a knife will not scratch it — and contains no copper; it is useful for Fire and Sulfur, not metal. Mica flakes glitter gold in stream sand but are feather-light. Green stains can be lichen or green clay: real copper minerals give a green flame. Many dark heavy rocks are just basalt: check the streak and the magnet.
Method 1: Panning
Panning uses water to wash light minerals away and leave the heavy ones. It finds cassiterite, magnetite, black sand and gold, and tells you which stream to follow upstream.
- Choose the spot. Dig where heavy minerals settle: the gravel on the inside of bends, just downstream of big boulders, and the bottom 10 cm of gravel on top of the bedrock.
- Fill the pan two-thirds with gravel and sand. Squat in water about 15 cm deep, flowing gently.
- Soak and break up. Sink the pan and knead the material with your fingers. Crush clay lumps; pick out and throw away large pebbles after rubbing them clean over the pan.
- Shake. Hold the pan level just under the water and shake it hard side to side for 10–20 seconds. This lets heavy grains sink to the bottom through the lighter sand.
- Wash off the top. Tilt the pan away from you, about 20°, and dip and lift it so the water sweeps off the top layer of light sand over the far rim. Level the pan and shake again. Repeat, shake–tilt–wash, until only a few spoonfuls are left.
- Read the tail. Swirl the last water slowly round the bottom. The heaviest grains trail behind in a dark "tail": black sand (test with your lodestone), brown-black cassiterite grains (heavy, non-magnetic, glassy, too hard to scratch with a knife), and any specks of gold.
Count what you get from each pan. If a stream gives a teaspoon of cassiterite per pan here and none 500 m further upstream, the source is in between. Once you have found it, Mining and Tunnelling gets the ore out and Ore Dressing: Jigs, Tables and Flotation separates it from waste rock in bulk.
Method 2: Roasting
Most ores improve if you roast them before smelting. Roasting means heating the ore in plenty of air, below melting. It:
- drives off water (bog iron, limonite) and carbon dioxide (siderite, malachite);
- burns sulfur out of sulfide ores (chalcopyrite, galena) as sulfur dioxide gas, turning them into oxides that can be smelted;
- cracks hard ore so it is easy to crush.
Step by step
- Break the ore to pieces the size of a walnut (2–4 cm). Pick out obvious waste rock (white quartz, grey country rock) by hand. Every kilogram of waste you remove now saves you fuel and trouble later.
- Build the heap on bare ground, out in the open and downwind of camp. Lay a bed of dry split hardwood about 20 cm deep, the size of the heap you want (1 m across for a first try).
- Layer it. Spread a layer of ore about 10 cm thick, then a layer of wood or charcoal fines, then ore, then wood — three or four layers, ending with wood. Leave gaps so air can get in.
- Light it at the bottom on the upwind side and let it burn. Iron ores need 2–4 hours of red heat. Sulfide ores need much longer — a large heap can smoulder for days, and serious copper sulfide ores were historically roasted several times over.
- Watch the heat. You want a dull red glow inside the heap at night (about 600–700 °C). If lumps start to look glassy, drip, or stick together, it is too hot — the sulfide is melting into a "matte" that seals the sulfur inside. Pull the heap apart a little to cool it.
- Check the result when cool. Roasted iron ore turns from brown or yellow to dark red-purple or black, often magnetic, and crumbles under a hammerstone. Roasted chalcopyrite loses its brassy shine and turns dull black-brown and earthy, and no longer smells of sulfur when crushed on hot coals.
- Crush and sort the roasted ore to the size the smelting chapter asks for — usually pea to hazelnut size (5–15 mm). Keep the fines separately.
Tip The magnetic roast test. Put a spoonful of crushed unknown red or brown ore in a covered clay pot with a spoonful of charcoal powder and leave it in a good fire for half an hour. If it comes out black and leaps to your lodestone, it is iron ore worth smelting.
How to tell it worked
- You can name the ore from its streak, heft, magnetism and flame, and two of these tests agree.
- Your panning tail is heavier and darker than the sand you started with, and grows richer as you move toward the source.
- Roasted ore is uniformly dark, crumbly, non-glassy, and has stopped smelling of sulfur.
Note Troubleshooting. Everything looks the same colour → you are looking at weathered surfaces. Break rocks open and wet them. Streak plate shows nothing → the mineral is harder than the plate (cassiterite, quartz). Crush a grain and look at the powder instead. Pan loses everything → you are tilting too steeply or not shaking long enough between washes. Roasted heap turned to a glassy lump → too much fuel, too little air. Use thinner fuel layers and smaller heaps.
Dangers
Danger Roasting and smelting fumes can poison you. Sulfide ores give off sulfur dioxide, a choking gas that burns the lungs. Ores containing arsenic (silvery-white arsenopyrite, which smells of garlic when struck or heated, and many grey copper ores) give off white arsenic smoke, which is a deadly poison (see Arsenic). Lead ores give fumes that slowly poison the brain, kidneys and blood — especially in children. Zinc ores give white fumes that cause a fever. Roast only in the open, stand upwind, keep children and animals away, never roast near food or water stores, and do not eat anything that grows on a roasting site.
- Falling rock. Do not dig under overhangs or into soft banks, and never enter old mine tunnels: rotten timbers, bad air and hidden shafts kill experienced miners.
- Cold water. Panning means hours in cold streams. Watch for numb hands and shivering; stop and warm up by a Fire.
- Flying chips. Breaking rock throws sharp fragments. Turn your face away, and if you can, wear a screen of thin leather or cloth over your eyes.
- Bogs. Bog ore lies in places that can swallow a person. Probe ahead with a long pole and never work alone.
What this unlocks
With ore in hand you can smelt Copper Smelting (from malachite, azurite and roasted chalcopyrite), alloy it with tin from cassiterite into Bronze, and smelt Iron (the Bloomery) from bog iron, hematite and magnetite. Galena leads to Lead; zinc ores, once you find them, to Zinc and Brass. Every smelting chapter needs forced air, so build Bellows next, and a good supply of Charcoal.
How it was first done
People used ore minerals long before they made metal. Red ochre (earthy hematite) was ground for paint more than 100,000 years ago, and malachite was used as a green pigment and eye cosmetic in Egypt and the Near East. The first metal worked was native copper, hammered into beads in Anatolia (modern Turkey) around 9,000–8,000 BC. When people later found that green malachite in a hot fire gave copper, the search for ores began in earnest; miners at Rudna Glava (in Serbia) were digging copper ore by about 5,000 BC, and at Timna (in the Negev desert) not long after. For most of history, prospecting was done exactly as described here: following green stains, rusty caps and heavy pebbles upstream.