◆ Rebuild

Part 3 · Metals

Axes, Chisels, Knives and Planes

Forge the essential cutting tools — axe, adze, chisels, knives, plane irons and scythe blades — from cheap iron with a thin edge of hard steel welded in, then harden, temper, handle and sharpen them so they hold an edge for years.

Difficulty
●●●●●
Time
A day for a chisel or a knife; two days for an axe with its handle; a week of practice before your edges are reliable
Steps from zero
13 prerequisites →

You need first

Steel

This unlocks

Doors, Windows and JoineryTimber Framing and Log BuildingStone CarvingFirewood and CoppicingButchery and MeatFruit Trees and OrchardsSickle, Scythe and Hand Harvest ToolsFurnitureRazors, Nail Clippers and Grooming ToolsWood Turning and TreenSharpening and HoningScissors, Shears and Folding KnivesPlanes, Drawknives and Woodworkers' Tools
The full path from nothing — 13 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. Charcoal
  9. Hides and Leather
  10. Bellows
  11. Iron (the Bloomery)
  12. Blacksmithing
  13. Steel
  14. Axes, Chisels, Knives and Planes

Do them roughly in this order. See it on the tech tree →

Why it matters

Stone axes fell trees, but slowly; bronze edges bend on knots; plain iron dulls in an afternoon. A steel edge — hardened, tempered and sharpened properly — cuts all day and comes back to razor sharpness in minutes on a stone. With a chisel and a plane you can make the tight joints of Timber Framing and Log Building, Furniture, barrels, boats, wagon wheels and the wooden frames of the The Lathe, The Loom and The Waterwheel. A scythe lets one person mow as much grain or hay as five with sickles (see Sickle, Scythe and Hand Harvest Tools).

This chapter assumes you can forge, forge-weld (Blacksmithing) and harden and temper steel (Steel). It shows how to put those skills together into the tools that every other trade depends on.

How it works

Every good edge tool solves the same problem: a hard edge breaks, a soft edge bends. The old answer is to use two metals.

  • The body is soft, tough wrought iron. It absorbs blows without cracking and is cheap — bloom iron is far easier to get than steel.
  • The edge is a thin piece of high-carbon steel (0.6–1.0% carbon) forge-welded onto or into the iron. Only this part is hardened.

This steeling saves precious steel, makes the tool almost impossible to snap, and speeds sharpening, because the stone mostly grinds soft iron. Almost every axe, chisel and plane iron made before about 1850 was built this way. Once steel is plentiful (Steel in Quantity), tools can be solid steel hardened only at the edge.

The second idea is the bevel, the angle ground on the edge. A thin angle cuts easily but crumbles; a thick angle survives hard blows but pushes through wood like a wedge. Match the angle to the job:

Tool Bevel Temper colour at the edge (see Steel)
Razor, carving knife 10–15° each side pale straw
Kitchen and work knife 15–20° each side straw
Wood chisel (paring) 25° on one side, honed at 30° straw
Mortise chisel, plane iron 25–30° on one side, honed at 30–35° straw to brown
Axe, hatchet 25–35° total, slightly rounded (convex) brown to purple
Adze 25–30° on one side brown to purple
Scythe, sickle very thin, made by hammering (peening) blue (soft enough to peen)

What you need

Item Notes
Forge, anvil, hammers, tongs See Blacksmithing. A 1–1.5 kg hammer for axes, 0.5–0.8 kg for chisels and knives
Wrought iron bar 10–15 mm thick, 40–50 mm wide for axes; 15–20 mm square for chisels
Steel High-carbon bar 4–8 mm thick, from carburising or sorted bloom (see Steel)
Hot chisel, punch, eye drift The drift is a tapered oval bar the shape of the axe eye, 2 × 4 cm at its fat end
Fine dry sand Welding flux
Quench tub 20 L or more of brine (one cupful of Salt per 4 L of water); a pot of oil or melted fat for thin blades
Grindstone Sandstone wheel 40–90 cm across on a cranked axle, with a water trough (see The Wheel and Axle)
Whetstones A coarse sandstone and a fine stone, flat, at least 15 × 5 cm
Leather strop A strip of hide glued to a flat board, dressed with fine abrasive powder
Handle wood Straight-grained ash, hornbeam, hickory, oak or elm, split (not sawn) and seasoned

Where to find it

  • Iron and steel: see Iron (the Bloomery) and Steel. Old salvaged springs and files are high-carbon steel and make excellent tool edges if you find them, but you do not need them.
  • Handle wood: straight young trees 10–20 cm thick of ash (grey diamond-patterned bark, leaves of 7–13 paired leaflets, black buds), hornbeam (smooth grey fluted trunk), hickory (North America), or the straight lower trunk of oak or elm. Split with wedges so the handle follows the grain; season the blanks 6–12 months under cover (see Basic Woodworking).
  • Grindstones: even-grained sandstone that does not crumble when wet. Rubbed with water and a scrap of iron, it should cut steadily without shedding loose grains.
  • Whetstones (hones): very fine-grained rocks — dark slate, grey-blue schist, the finest sandstones, or white, waxy novaculite. Look in stream beds for flat pebbles that feel smooth as soap. Rubbed wet on iron, a good hone quickly makes a grey slurry and leaves fine, even scratches. See also Abrasives and Grinding Stones.

Method 1: The axe

The classic European and Scandinavian axe has a wrapped eye: a flat iron bar is folded around a drift, the two ends are welded into the blade, and a steel bit is welded into the edge. It needs no big punch and wastes no metal.

1 Thin the middle 2 Fold round drift 3 Weld, insert steel 4 Finished head bar seen from the edge seen from above seen from above side view Middle 8 cm drawn ⅔ as thick hatchet: 12 × 40 mm, 22 cm long felling axe: 15 × 50 mm, 26 cm long Drift in the eye oval 2 × 4 cm Arms meet beyond the eye Cheeks welded eye outward Eye kept open Steel wedge in split ends, 1–1.5 cm proud Steel bit hardened Iron soft, tough wedged handle
Fig. 1 Forging a wrapped-eye axe. The bar is folded around the drift, the cheeks are welded, the blade is split, and a steel bit is welded into it.

Sizes. For a hatchet (about 0.8 kg) use iron bar 12 × 40 mm, 22 cm long. For a felling axe (about 1.5 kg) use 15 × 50 mm, 26 cm long. The steel bit is a wedge 3–4 cm deep, as wide as the finished edge (8–11 cm), tapering from about 6 mm to 2 mm.

  1. Thin the middle 8 cm of the bar to about two-thirds its thickness. This becomes the eye.
  2. Fold. Heat the middle to yellow, bend the bar into a U, put the drift in, and hammer the arms together round it until they meet. The eye should be an oval about 2 × 4 cm for a hatchet, 2.5 × 5 cm for a felling axe.
  3. Weld the cheeks. Scarf the inside faces of the arms slightly, flux with sand, and weld them together from the eye outward, leaving the last 3–4 cm unwelded. Drive the drift back in after each heat so the eye does not collapse.
  4. Prepare the bit. Forge the steel wedge and file its faces bright.
  5. Insert the bit. Open the unwelded ends slightly with a hot chisel, flux, and push the steel wedge in so that 1–1.5 cm of it sticks out beyond the iron. Squeeze the jaws shut on it with a few blows.
  6. Weld the bit. Bring it slowly to welding heat — steel burns at a lower heat than iron, so stop at light yellow, not white, and keep plenty of charcoal over it. Weld with light blows first, then firm ones. Take a second welding heat to be sure.
  7. Shape the blade. At orange heat, draw out the blade, flaring it toward the edge. Forge the edge down to about 1.5–2 mm thick. Keep the cheeks just behind the edge slightly convex, so the axe splits chips away instead of sticking.
  8. Dress the eye. Drive the drift in from both sides at orange heat. A slight hourglass shape (eye wider at top and bottom than in the middle) lets the wedge lock the handle.
  9. Normalise three times: heat the whole head to cherry red and let it cool in still air.
  10. Grind the bevel roughly, leaving the edge 1 mm thick.
  11. Harden only the bit. Heat the front 4–5 cm to an even cherry red (until a lodestone no longer sticks). Quench edge down in brine to a depth of 3 cm, moving it up and down, until it stops hissing; then plunge the whole head.
  12. Temper. Polish both cheeks bright with sandstone. Lay the head on a red-hot bar, or heat the eye end gently over the fire, and let the colours run toward the edge. Quench when the edge turns brown going to purple.

Easier first axe: punch and drift an eye through a block 4 × 4 × 10 cm, 2 cm from one end, draw the rest into a blade and weld on a steel bit. More hammering, fewer welds.

The adze is forged like an axe, but with the blade turned 90° to the handle and gently curved. The bevel goes on the top (handle) side; the underside is flat. It flattens beams and hollows troughs and canoes.

Method 2: Chisels and plane irons

On a chisel or a plane iron, the steel goes on the flat face (the back), with the bevel ground through the iron behind it. That way the hard steel is right at the cutting edge and the soft iron supports it.

Axe bit section across the blade Chisel side view Plane iron in its wooden body Knife section across the blade iron steel 25–35° total slightly convex; steel inserted in a split iron body 25–30° steel on the flat back Bevel on top back dead flat; hone a 30° micro-bevel 45° wedge mouth 1–2 mm Bevel down steel on the upper face, right at the cutting edge iron steel iron 15–20° a side grinding exposes the steel at the edge
Fig. 2 Where the steel goes. Dark is hardened steel, grey is soft iron. Each tool puts its steel where the edge meets the wood.

A firmer chisel (the general-purpose wood chisel, 6–38 mm wide):

  1. Forge an iron bar about 15 × 8 mm into a blade 12–15 cm long, with a square tang 8–10 cm long tapering to a point.
  2. Weld a strip of steel 2–3 mm thick and 5–6 cm long onto the face at the cutting end, at a light yellow heat.
  3. Forge to width, keeping the back dead flat and the blade tapering to 3–4 mm at the edge.
  4. Normalise, grind the back perfectly flat and the bevel to 25°.
  5. Harden the front 3 cm in brine or water, and temper to straw.

A mortise chisel is the same but thick (10–15 mm) and narrow, for chopping deep holes with a mallet; temper it to brown. A plane iron is a blade 45–55 mm wide, 15–20 cm long and 3–5 mm thick, steeled on the flat face, hardened at the bottom 3 cm and tempered to straw.

The plane body is a wooden block that holds the iron at a fixed angle, so it can only take a thin, even shaving.

Plane Body length Use
Jack plane 35–45 cm First, rough flattening
Smoothing plane 20–25 cm Final finish
Jointer 55–75 cm Making long, straight edges for joining boards
  1. Take a seasoned block of beech, hornbeam, oak or fruitwood about 7 × 7 cm and the length you want.
  2. Chisel a wedge-shaped throat down from the top, with a flat, true bed for the iron sloping at 45° to the sole, a third of the way from the front, and two narrow abutments in the side walls for the wedge.
  3. Open the mouth in the sole so the gap in front of the edge is only 1–2 mm; a tight mouth stops the wood tearing ahead of the cut.
  4. Hold the iron with a hardwood wedge. Tap the iron to deepen the cut; tap the back of the plane to loosen it.
  5. Rub the sole flat on sandstone.

Method 3: Knives

The simplest knife is in Blacksmithing. For a better one, laminate:

  • Inserted edge. Forge an iron blank, split its edge with a hot chisel, weld in a strip of steel 2–3 mm thick, exactly as for the axe.
  • Sandwich ("three layers"). Weld a steel strip 3–4 mm thick between two iron strips each 2–3 mm thick. Forge the knife from this bar; when you grind the edge, the steel core is exposed down the middle.

Normalise three times, harden in warm oil or fat (thin blades crack in water), temper to straw, and hone at 15–20° each side. Burn the heated tang into a hardwood or antler grip, or rivet wooden scales to a full-width tang (see Nails, Rivets and Wire Fasteners).

Method 4: Scythe and sickle blades

A scythe blade is the hardest edge tool to make by hand: a blade 60–90 cm long but only 1.5–2.5 mm thick, with a raised rib along its back to stiffen it and a tang bent up at about 70° to fix it to the long handle (the snath). Make sickles first.

  1. Sickle: forge steel, or iron with a steel edge, into a curved blade 30–45 cm long, 25–35 mm wide and 2–3 mm thick. A serrated edge, cut with a chisel like a coarse file (see Files and Saws), stays sharp far longer in grain.
  2. Scythe: draw out a heavy bar a hand-width at a time, turning up the back 4–6 mm as the rib. Expect your first to be heavy and wavy.
  3. Heat treat: harden in oil or fat and temper evenly to blue, soft enough to peen.
  4. Peening: hammer the last 3–5 mm of the edge cold, with light overlapping blows on a small narrow-faced anvil, until it is as thin as paper. This thins and work-hardens it. Re-peen every few days of mowing; hone every few minutes with a stone carried in a water holder on the belt.

Handles and hafting

  • Axe handles: 35–45 cm for a hatchet, 75–90 cm for a felling axe (about armpit to fingertips). Split the blank so that, looking at the end of the handle, the growth rings run in line with the blade. Carve it to fit the eye tightly from below, coming through 1–2 cm.
  • Wedging: split a slot down the end two-thirds the depth of the eye, drive the head on, and drive in a dry hardwood wedge smeared with glue or resin. A small iron wedge across it locks it further. Sight down the handle: the edge should line up with its centre.
  • Chisel and knife handles: burn the red-hot tang into a pilot hole in a hardwood handle, then drive it home cold. An iron or copper ring (ferrule) round the wood stops it splitting.

Sharpening

Sharpening has three stages: grind the shape, hone the edge, strop off the burr. Sharpening and Honing covers each tool in more detail.

Top of the stone moves into the edge about one turn a second Tool held at its bevel angle, dipped in water often Sandstone 40–90 cm across Crank Water trough drain it after use Axe handle, seen from the end edge ↔ back edge ↔ back Strong rings along the blade Weak rings across it Hone bevel flat, back lifted a hair; edge leading Strop leather on a board; edge trailing
Fig. 3 Sharpening. Grind on a slow, wet sandstone wheel turning into the edge; then hone on a fine stone and strop on leather. Below, the right way to orient the grain of an axe handle.
  1. Grind. Turn a wet sandstone wheel slowly — about one turn a second — with the top moving into the edge. Hold the tool at its bevel angle and move it across the wheel, dipping it in water often. If the steel turns straw or blue, you have spoiled the temper; grind that part away and go gentler. Stop when a tiny rough lip, the burr, can be felt along the whole edge on the side away from the bevel (slide your thumb across the edge from the back, never along it).
  2. Hone. Lay the bevel flat on a wet fine stone, lift the back a hair, and rub. Then give the flat back a few strokes to turn the burr over. Repeat, lighter each time.
  3. Strop. Pull the edge, trailing, over leather dressed with very fine abrasive — powdered red hematite ("rouge") or fine wood ash. Ten strokes a side removes the last burr.
  4. Store tools dry and lightly greased.

How to tell it worked

  • The light test. Hold the edge toward a bright window or the sky and look straight down at it. A sharp edge is invisible. Dull spots and nicks shine as bright points or lines.
  • The thumbnail test. Rest the edge on your thumbnail at a low angle without pressure. A sharp edge bites and catches; a dull one slides.
  • End grain. A sharp chisel or plane pares a thin, unbroken curl from the end grain of softwood. A dull one crushes and tears it.
  • The axe should bite deep into green wood and throw out large chips, not bounce. After a day of chopping, the edge should still shave the wood smoothly.
  • The file test (see Steel): a file should barely touch the edge, but bite easily into the cheeks and eye.

Note Troubleshooting. Bit came loose or shows a dark line → a bad weld. Clean both surfaces bright, flux generously, and weld at a slightly lower heat with more charcoal over the work; steel burns easily. Edge chips in use → too hard. Temper one colour further (straw → brown, brown → purple), or grind a thicker bevel. Edge rolls over or dents → too soft, or the "steel" was iron. Check with the spark test and re-harden. Cracks along the edge after quenching → edge was too thin or overheated, or the quench was too harsh. Leave 1 mm at the edge before hardening; try warm brine or oil. Plane chatters or tears the wood → iron loose on its bed, mouth too wide, or edge dull. Flatten the bed, glue a patch in front of the mouth to close it, and resharpen. Axe head keeps working loose → the handle was green and shrank. Use wood seasoned six months or more.

Dangers

Danger Flying axe heads. A loose head can fly off on the backswing with enough force to kill. Check the wedge before every use. Never swing an axe with anyone within two handle-lengths of you, in any direction, and clear twigs and vines that could catch the swing.

Danger Bursting grindstones. A large stone wheel spun too fast, or one with a hidden crack, can fly apart. Turn it by hand, no faster than about one turn per second for a 60 cm wheel; ring it with a light tap before mounting — a cracked stone sounds dull — and never stand directly in line with its face. Never let it stand half in water: the soaked side becomes heavy and soft, and the stone runs out of balance.

  • Cuts. Most edge-tool injuries come from sharpening and carrying, not from use. Carry axes and chisels with a leather or wooden guard over the edge. Always cut away from your body and your other hand.
  • Glancing blows. A dull axe bounces off the wood toward your legs. Keep it sharp, chop with your feet apart, and let the bit land beyond your feet, not between them.
  • Quench oil fires and shattering steel — see Steel.

What this unlocks

With good edge tools, woodworking leaps forward: Timber Framing and Log Building, Furniture, Barrels and Cooperage, Boats and Sails, Wagons and Carriages and waterwheels. The same skills make Files and Saws, kitchen knives and cleavers (Kitchen and Cooking), shears, the moulding planes, gouges and augers of Planes, Drawknives and Woodworkers' Tools, and the cutting tools of the The Lathe and Machine Tools. A scythe and sickle multiply what each farmer can harvest (Sickle, Scythe and Hand Harvest Tools).

How it was first done

Iron axes with welded steel edges were common across Europe and the Near East by Roman times; the Romans made a wide range of chisels, planes, adzes and drawknives that look almost exactly like tools of 1900. The wooden plane with an iron blade is a Roman invention, or at least was first widespread under Rome; examples survive from Pompeii and from Roman Britain and Germany. The scythe with a long blade appears in Roman-era Europe and became the main harvesting tool of northern Europe in the Middle Ages. Japanese smiths carried the laminated-steel tradition to its peak in their chisels, plane irons and kitchen knives, which are still made by forge-welding hard steel to soft iron. In Europe and America, solid cast-steel tools replaced laminated ones during the 1800s, once crucible and then Bessemer steel became cheap.

Source: content/entries/metals/edge-tools.md