◆ Rebuild

Part 8 · Chemistry

Laboratory Glassware

How to turn molten glass into the tools of chemistry — drawn tubing, bent tubes, flasks, retorts, test tubes, beakers, condensers and measuring vessels — and how to seal, join, heat and care for them. With a shelf of glass, a spirit lamp and a balance you have a real laboratory.

Difficulty
●●●●●
Time
A day at the furnace for a stock of tubing and flasks; an evening per small lampworked piece; weeks to master
Steps from zero
7 prerequisites →

You need first

Glass

This unlocks

Fluorspar and Fluorine CompoundsHydrogen, Oxygen and GasesBurners, Stands and Laboratory EquipmentOrganic Synthesis and Fine ChemicalsPhosphorusIdentifying SubstancesScientific Glassblowing and Glass-to-Metal SealsThe Vacuum PumpCulturing MicrobesInsulin (Overview)Medical InstrumentsPharmacy: Tablets, Capsules, Ointments and InhalersThe BarometerPhotographyThe Thermometer
The full path from nothing — 7 steps before this one
  1. Fire
  2. Finding and Preparing Clay
  3. The Kiln
  4. Pottery
  5. Lime
  6. Lye and Potash
  7. Glass
  8. Laboratory Glassware

Do them roughly in this order. See it on the tech tree →

Why it matters

Clay soaks things up and hides what happens inside; metal is eaten by acids. Glass is clear, smooth, non-porous, and almost nothing attacks it except hydrofluoric acid and hot strong alkali. That is why chemistry is done in glass.

With the pieces in this chapter you can:

This chapter starts where Glass ends: you can melt glass in a crucible, blow it on an iron pipe and anneal it. Now you shape it for the laboratory.

How it works

Glass has no melting point. As it warms it softens gradually, from rigid to taffy to honey:

Glass is… Ordinary soda-lime glass Colour of glow
Hard, but can crack from uneven heat below 500 °C none
Annealing — stresses relax about 520 °C faint dull red, seen only in shade
Soft enough to bend and sag 650–750 °C dull to cherry red
Soft enough to draw, blow and seal 800–1,000 °C bright orange

So you can rework cold glass — bend it, seal it, draw it thinner — just by heating a small part of it in a hot flame. This is called lampworking, and it is how most laboratory glass was shaped until the 1900s. The full craft, with hotter burners and complex joins, is in Scientific Glassblowing and Glass-to-Metal Seals.

Why glass cracks. Glass expands when hot. If one part is hot and the next part cold, the hot part pushes and the glass breaks — this is heat shock. Two rules follow: heat and cool every piece gradually and evenly, and make laboratory glass thin and even-walled, because a thin wall has less difference between its two faces. Thick glass is weaker in a flame, not stronger.

Borosilicate. Ordinary glass expands about three times as much as glass made with boron (from the mineral borax). Low-expansion borosilicate glass can go from flame to cold water without cracking. It is the glass of modern laboratories — but it melts at about 1,600 °C, hotter than a charcoal crucible furnace can reliably reach. See Going further.

What you need

Item Details
Glass furnace and blowpipes As in Glass — for gathering, drawing tubing and blowing flasks
Molten glass A crucible of well-fined glass. The soda-lime recipe (best: softest, most even) or potash-lime. Avoid lead glass for chemistry
A hot small flame A spirit lamp (below) for thin tubing; an oil lamp or a small charcoal fire blown by a mouth blowpipe or Bellows for anything bigger
Scoring tool A file of hardened steel (Files and Saws), a sharp flint flake, or a shard of emery or corundum (Abrasives and Grinding Stones)
Tools Wooden paddles, tongs and a flat marver stone (Glass); a charcoal block or iron rod to push soft glass
Annealing pot A clay pot of hot wood ash, or the annealing oven from Glass
Fine abrasives Fine sand, then emery powder, with water — for grinding stoppers
Cork, beeswax, clay, linseed oil For stoppers and seals
Balance For graduating vessels (Measurement from Scratch)

The spirit lamp

Make a small glass or glazed clay bottle, about 100–200 ml, with a narrow neck. Push a wick of loose cotton or linen threads through a short tube of clay, glass or sheet metal set in the neck so the wick cannot slip down. Fill with strong spirit — at least 80 % alcohol, from Distillation. It burns with a clean, sootless, nearly invisible blue flame that does not blacken glass. Keep a cap on it when not in use, or the spirit evaporates and the wick dries out.

A spirit lamp alone will soften thin soda-lime tubing (walls under 1 mm, under 8 mm across). For more heat, blow its flame sideways with a mouth blowpipe — a thin tube about 20 cm long with a fine tip — breathing in through your nose and blowing steadily out through puffed cheeks. Old glassworkers used a tallow or oil lamp with a large wick and a foot bellows feeding the jet.

Where to find it

  • Glass materials — sand, potash or soda, and limestone: see Glass, Lye and Potash and Soda Ash and Baking Soda.
  • Borax forms white crusts and beds in dry lake basins and around hot springs in deserts and high plateaus — Tibet (the old source, traded to Europe as tincal), Turkey, the western United States, the Andes of Chile, Argentina and Bolivia. It is soft, white, sweetish-alkaline in taste, dissolves fairly easily in hot water, and on a hot coal swells up into a white froth and then melts into a clear glassy bead.
  • Cork is the thick, spongy bark of the cork oak of the western Mediterranean — Portugal, Spain, North Africa. It can be stripped from a living tree every 9–10 years without killing it. Elsewhere, use waxed softwood or ground-glass stoppers.
  • Beeswax for sealing: see Beekeeping.

Method 1: Drawing tubing

Tubing is the most useful single form of laboratory glass: you make test tubes, droppers, jets, burettes, condensers and connections from it. Glassworks drew it by the hundred metres in one go.

1. Gather, marver, blow a small bubble 2. A helper sticks a punty to the far end 3. Both walk backward, turning their irons — the bubble stretches into a tube Air bubbleabout ⅓ of the width Blowpipe Puntysolid iron rod with a hot gob walk backward walk backward Thinnest, most even tubing in the middle walk faster = thinner tube · stop when it stiffens (a few seconds) Wooden slats10–20 m of them Cut end wall about ⅒ of the width
Fig. 1 Drawing tubing. A thick bubble is blown on the pipe, a helper attaches a punty to the far side, and the two walk apart. The bubble stretches into a long tube; the air inside it becomes the bore.
  1. Prepare the floor. Lay a line of wooden slats or boards, 10–20 m long, on the floor beside the furnace, about a hand-width apart. The hot tube will rest on them; they char a little but do not stick.
  2. Gather. Gather a lump of glass the size of an orange (about 0.5 kg) on the blowpipe, in two or three dips, letting each cool a moment before the next.
  3. Shape a cylinder. Roll it on the marver into a fat, even cylinder about 8–10 cm long.
  4. Blow a bubble. Blow a small bubble inside it — the hollow should be about a third of the width. A small bubble gives thick-walled tubing; a large bubble, thin-walled. For laboratory tubing, aim for walls about a tenth of the outside width.
  5. Reheat the whole gather to an even bright orange.
  6. Attach the punty. A helper brings a punty with a small gob of hot glass on its tip and presses it onto the far end of the gather, so it sticks.
  7. Walk apart. Both people walk steadily backward away from each other, keeping the tube level and turning their irons slowly. The gather stretches into a tube. Walk fast for thin tubing, slowly for thick. The blower can puff gently from time to time to keep the bore open.
  8. Lay it down on the slats once it has stiffened — within a few seconds. Thin tubing cools evenly and needs little annealing; tubing thicker than 1.5 cm across should be cut into lengths and annealed.
  9. Cut it into lengths of 50–100 cm when cool (Method 2) and sort it by width. Keep pieces of the same width together.

The tube is widest near the ends and thinnest in the middle; the even middle part is best for small work.

Rods. Do exactly the same without blowing a bubble, and you get solid glass rod — for stirring rods and for drawing out tips.

Method 2: Cutting, polishing and bending

1. Cut: one scratch, then snap 2. Bend: heat a wide band, turning 3. Draw a jet: soften, then pull apart 4. Test tube: seal the end, blow it round Scratch, wetted⅓ of the way round Thumbs behind the scratchpull apart and bend away from it turn constantly Heated band 5–8 cm3 × the tube width bend when it sags round, not kinked pull outside the flame Jet or droppercut the neck to the width you need pull off the tail heat and blow gently Test tubebottom as thin as the walls; flare the rim
Fig. 2 Working tubing in a flame. Score and snap to cut; turn the end in the flame to smooth it; heat a broad band while rotating and bend once it sags; pull a softened tube apart to draw a jet, or seal one end to make a test tube.

Cutting

  1. Make one firm scratch across the tube with the edge of a file or flint, about a third of the way round. Do not saw back and forth.
  2. Wet the scratch with a drop of water or spit.
  3. Hold the tube with both thumbs together behind the scratch, on the opposite side. Pull your hands apart and bend gently away from the scratch. It snaps cleanly.
  4. Wide tubes, flasks and bottles: after scratching, touch the scratch with the red-hot tip of a glass rod or an iron wire. The heat makes a crack run from the scratch. Lead it round with the hot tip, a little ahead of the crack.

Fire-polishing

Fresh-cut glass is as sharp as a knife. Warm the end gently above the flame, then turn it in the hottest part until the edge rounds and glows dull red. Do not overdo it — the end will start to close.

Bending

  1. Warm the tube gently above the flame, then hold the middle part in the flame and turn it constantly, like a spit roast, with both hands.
  2. Heat a band 5–8 cm long — about three times the width of the tube. A spirit lamp's flame is too narrow: move the tube slowly back and forth along the flame, or spread the flame with a flat fishtail-shaped tip.
  3. When the glass feels soft and starts to sag under its own weight, take it out of the flame and bend it smoothly in one movement to the angle you want, keeping both arms in one plane.
  4. A good bend keeps the same roundness all the way round. A flattened or kinked bend was too narrow a heated band, or bent too fast; it will be weak and will block flow.
  5. Hold the bent piece in a smoky (yellow, sooty) flame for a moment to coat it with soot, then set it on a warm bed of ash to cool slowly. This is a quick anneal.

Drawing jets, droppers and pipettes

Heat a band of tubing until soft, take it out of the flame and pull the two ends apart steadily. The middle draws down into a thin neck. Let it cool, then cut the neck at the width you want. The result is a jet for a burette, a dropper (fit a small bladder or teat on the wide end) or a pipette — a tube you fill by sucking to a mark. Never suck up acids or anything poisonous with your mouth — fill pipettes by dipping and closing the top with a finger, or use a bulb.

Sealing and test tubes

  1. Take a 15–20 cm length of tubing 1.2–2 cm across. Heat the middle while turning, as for drawing, and pull it apart: you now have two tubes, each closed with a thin tail.
  2. Heat the tail end and pull off the extra glass with a glass rod or tongs, so it closes.
  3. Heat the closed end until it is soft and slightly thickened, then take it out and blow gently into the open end to round it. Make the bottom the same thickness as the walls — a thick bottom cracks in a flame.
  4. Fire-polish the open end and flare it slightly with a charcoal cone or an iron rod so a stopper fits.
  5. Anneal in warm ash.

Method 3: Flasks, retorts and beakers

These are blown at the furnace, as in Glass.

  • Round-bottomed flask. Blow a round bubble of thin, even wall (1–2 mm) on the pipe, keeping it turning. Leave a neck 10–15 cm long and 2–3 cm across. Crack it off and fire-polish the neck. Round flasks take heat best and are the shape to use for boiling and distilling. Sizes from 100 ml to 2 litres.
  • Flat-bottomed flask. As above, but press the bottom gently on the marver while soft so it stands. Good for storage and for mixing, less good for strong heat.
  • Retort. Blow a round flask. Reheat the neck just above the bulb, and while it is soft, bend it downward to about 60° with tongs or by tilting the pipe, so it slopes away from the bulb. The long neck itself acts as an air condenser. A tubulated retort has a second short neck on top, with a stopper, so you can add the charge without taking it apart: make it by blowing a small extra bump on the bulb and opening it with a hot iron.
  • Receiver. A round flask with a wide neck that takes the end of the retort.
  • Beaker. Blow a straight-sided cylinder with a flat bottom. Crack off the top (score and hot wire), fire-polish the rim, and while the rim is soft, pinch a small spout with tongs.
  • Funnels and bottles are blown the same way; glazed stoneware funnels work just as well.
Round flaskboiling, distilling Flat-bottomed flaskmixing, storing Retortdistilling acids Beakerdissolving, rough measuring cold water in, low end water out, high end vapour Test tubesmall tests Funnel + paperfiltering Liebig condensertilt it so the liquid runs down Spirit lampclean, sootless flame
Fig. 3 A basic set of laboratory glass, and what each piece is for.

Method 4: Measuring vessels

Glass is only useful for measuring once it is marked. You calibrate with water, because 1 ml of water weighs 1 g (close enough at room temperature).

  1. Set the vessel on a level surface beside your balance (Measurement from Scratch).
  2. Weigh water into it 5 or 10 g at a time. At each step, look at the water level at eye height and mark the bottom of the curved surface.
  3. Mark with a scratch from a hard stone, a file, or a diamond-hard shard of corundum. For clearer marks, cover the glass in a thin coat of beeswax, scratch the lines through the wax, and rub a paste of soot and oil into them.
  4. Make a measuring cylinder marked every 1–5 ml, measuring flasks with one mark at exactly 100 or 1,000 ml (for standard solutions), a burette (Acids, Bases and Testing) and 10 ml pipettes.

Method 5: Stoppers and joints

  • Cork. Boil cork for a few minutes to soften it, then cut and roll it to fit. To bore a hole for a tube, use a red-hot iron rod or a sharpened thin metal tube turned like a drill. Cork is fine for water, alcohol and gases, but strong acids char it and nitric acid eats it.
  • Waxed wood. Turn a tapered stopper from soft, close-grained wood (The Lathe) and boil it in beeswax. Fine for water, oils, lye; not for strong acids.
  • Ground-glass stoppers — the only seal that suits every chemical:
    1. Make a solid tapered glass stopper slightly larger than the neck — a taper of about 1 in 10 (the stopper narrows by 1 mm for every 10 mm of length).
    2. Grind the inside of the neck and the stopper together with a paste of fine sand and water, turning the stopper back and forth and lifting it often to spread the paste.
    3. Change to fine emery (Abrasives and Grinding Stones) and keep grinding until both surfaces are an even, frosted grey with no clear patches. Usually 30–60 minutes.
    4. The ground pair now seals with a smear of grease or wax, or dry for acids. Keep each stopper with its own bottle — tie them together.
  • Lutes are pastes that seal joints:
Lute Recipe Use
Clay and sand 1 part clay, 1 part fine sand, water to a stiff dough Acids, high heat; cracks if moved
Fat lute Fine dry clay worked with boiled linseed oil to a putty Acid fumes; stays soft for weeks
Flour paste Flour and water Alcohol and water only — acid chars it
Lime and egg white Slaked lime kneaded with egg white Quick-setting, water and steam
  • Flexible joints. Join glass tubes end to end with a sleeve of cleaned animal gut or bladder, tied with thread, for gases and water. Later, rubber tubing (Rubber) is far better.

The condenser

A Liebig condenser cools vapour to liquid in a small space:

  1. An inner tube 50–60 cm long, 1–1.5 cm across.
  2. Over it, a wider tube (3–4 cm across) about 10 cm shorter, closed at each end by a bored cork or a ring of bladder tied tight round the inner tube.
  3. Two short side tubes in the outer one — one near each end. Cold water goes in at the lower end and out at the upper end, so the coldest water meets the vapour last, and the jacket stays full.

A simpler version: wrap the inner tube in wet cloth and keep pouring cold water over it.

Heating glass safely

  • Never put a naked flame against a flask. Stand it on a sand bath (an iron or clay dish of fine sand over the fire), in a water bath (never above 100 °C), or on a pad of iron wire gauze.
  • Warm and cool slowly. Never set hot glass on a cold stone or wet surface, never heat glass empty or above the liquid level, and never add cold liquid to hot glass.
  • Never heat a closed vessel, and point test tubes away from everyone — liquids bump and spurt.

How to tell it worked

  • The warm-water test. A new flask should survive being filled with water at 50 °C, then 80 °C, then boiling. If it cracks, it was uneven, too thick, or badly annealed.
  • Stoppers should hold water in an upside-down bottle overnight without a drop.
  • Joints should hold when you blow gently into the apparatus with all exits closed, and a dab of soapy water on each joint shows no bubbles.

Note Troubleshooting. Tubing collapses into a rod → the bubble was too small, or the glass too hot; puff into it while drawing. Bends kink → heat a longer band, turn more evenly, and bend more slowly. Cracks appear hours after working → not annealed. Soot-anneal and cool in warm ash. Flask cracks on first heating → wall too thick or uneven, or heated directly. Use a sand bath, blow thinner. Ground stopper sticks fast → warm the neck gently and quickly (so it expands before the stopper), then tap with wood.

Dangers

Danger Hot glass looks exactly like cold glass. Glass stays hot enough to burn deeply long after it stops glowing. Set hot pieces in one marked place, and touch every piece to the back of a finger lightly before gripping it.

Danger Cut glass and splinters. Fire-polish every cut end and wear eye protection when cutting. Hold tubes in a cloth when snapping them or pushing them into a cork — the classic laboratory injury is a tube snapping and driving into the palm. Wet the tube, hold it close to the cork, and twist rather than push.

  • Bursting flasks. Inspect every piece against the light before use; throw away anything with a crack or star-shaped chip.
  • Never breathe in through any tube used in a flame or in chemistry. Blow only.
  • Spirit lamps spill burning spirit that is nearly invisible in daylight. Refill only when cold and out; smother a lamp fire with a damp cloth or sand.
  • Broken glass goes in one closed pot — it is good cullet for the next melt (Glass).

Going further

How it was first done

Glassblowing began in the Roman world in the 1st century BC, and alchemists in Roman Egypt already distilled in glass. Islamic glassmakers and alchemists of the 8th–13th centuries made the alembics, flasks, retorts and receivers whose shapes lasted a thousand years, and Venetian and Bohemian glasshouses supplied Europe's apothecaries from the 1400s.

Lampworking — shaping tubing in a lamp flame blown by a bellows or mouth blowpipe — was practised in Venice and Nevers in the 1600s and became the trade of the scientific glassblower. The water-jacketed condenser was described by Christian Ehrenfried Weigel in 1771 and later made famous by Justus von Liebig. Ground-glass joints were made by hand for centuries; standard interchangeable joints arrived only in the 1920s. Borosilicate laboratory glass was developed by Otto Schott in Jena in the 1880s and 1890s, and the American company Corning sold it as Pyrex from 1915.

Source: content/entries/chemistry/lab-glassware.md