◆ Rebuild

Part 8 · Chemistry

Making Photographic Papers and Plates

Turning a kitchen-scale silver emulsion into a steady supply of plates and paper. Slow chloride and fast bromide emulsions in gelatin, ripening for speed, washing and finishing; the levelling slab and drying cupboard for glass plates; the barium-white baryta layer and the coating trough for paper; coating by machine in outline; and testing every batch for speed, contrast and fog so a photographer can trust it.

Difficulty
●●●●●
Time
An evening for a test batch of emulsion; a day to coat and two to dry; a month of test batches before the results are steady
Steps from zero
34 prerequisites →

You need first

PhotographySilver Nitrate and Silver SaltsGelatin

This unlocks

—
The full path from nothing — 34 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Sulfur
  7. Hunting and Trapping
  8. Basic Woodworking
  9. The Kiln
  10. Pottery
  11. Charcoal
  12. Hides and Leather
  13. Lime
  14. Tar, Pitch and Glue
  15. Lye and Potash
  16. Glass
  17. Bellows
  18. Saltpeter
  19. Glues and Adhesives
  20. Copper Smelting
  21. Lead
  22. Iron (the Bloomery)
  23. Laboratory Glassware
  24. Sulfuric Acid
  25. Lenses
  26. Gold and Silver
  27. Blacksmithing
  28. Nitric Acid
  29. Steel
  30. Silver Nitrate and Silver Salts
  31. Photography
  32. Axes, Chisels, Knives and Planes
  33. Butchery and Meat
  34. Gelatin
  35. Making Photographic Papers and Plates

Do them roughly in this order. See it on the tech tree →

Why it matters

The Photography chapter makes a few plates at a time in a dish. That proves the process, but a camera user, an X-ray room, a printing works or a survey team needs hundreds of plates and sheets of paper that all behave the same. If one batch needs 2 seconds and the next 20, every picture becomes a guess.

This chapter is the bridge from a craft to a supply:

The same emulsion coated on plastic becomes film (Photographic Film Base).

How it works

An emulsion is not really an emulsion; it is a jelly with tiny crystals of silver salt spread through it. Pour silver nitrate into a warm gelatin solution that holds a bromide or chloride, and silver bromide or chloride forms as crystals a fraction of a micrometre across. Gelatin keeps them apart so they do not clump and settle, soaks up the bromine that light sets free, and lets developer reach every crystal.

Which salt.

Salt Speed Contrast Use
Silver chloride Very slow High; blue-black or warm tones Gaslight (contact) paper, lantern slides, copying
Chloride and bromide mixed Slow to medium Medium; warm brown-black Warm-tone enlarging paper
Silver bromide Fast Medium Bromide paper, plates
Bromide with 2–4 % iodide Fastest Lower Camera plates and film

Ripening. Fresh crystals are tiny, slow and contrasty. Kept warm in the emulsion, especially with excess bromide or ammonia present, small crystals dissolve and large ones grow. This physical ripening makes the emulsion faster and softer (less contrasty) and, carried too far, foggy and grainy. A second warming after washing, the after-ripening, lets traces of sulfur compounds in the gelatin form specks of silver sulfide on the crystals. These specks are where the latent image starts, and they can raise the speed several times.

Always excess halide. There must always be a little more bromide or chloride than the silver can use, about 15–25 % more. Free silver nitrate in a developing emulsion gives fog. (Old printing-out papers did the opposite, on purpose, but they are not developed.)

Gelatin matters. Two gelatins that look the same can give emulsions of very different speed, because of the traces of sulfur they carry. Buy or make gelatin in large lots, test each lot, and keep the good one for emulsions (Gelatin).

What you need

Item Amount for one batch Notes
Silver nitrate, pure 10–30 g Silver Nitrate and Silver Salts
Potassium bromide 8–26 g Bromine and Bromides
Potassium iodide 0.3–0.6 g From seaweed, Iodine
Salt (pure, for chloride emulsions) 4 g Recrystallised Salt
Photographic gelatin, tested 20–60 g Gelatin
Ammonia water (for fast plates) 10 ml Ammonia
Chrome alum A pinch, as solution Hardener; Chromium and Its Compounds
Alcohol 20–30 ml Helps spreading; Distillation
Distilled or rain water 20 litres per batch Tap and well water carry chloride and iron
Water bath with thermometer Held at 40–55 °C; The Thermometer
Glass, glazed or enamelled vessels, glass rods Never bare iron, copper or brass
Coarse canvas or a perforated glass plate For noodling
Glass plates, cut and edged Window Glass
Rag paper and barium sulfate For paper; below
Darkroom with deep red and amber safelights The Darkroom and the Enlarger

Where to find it

  • Silver from native silver or cupelled lead (Gold and Silver), dissolved as in Silver Nitrate and Silver Salts. Recover every gram from scraps and spent fixer.
  • Bromide from bittern, the liquor left after salt-making (Bromine and Bromides); iodide from the ash of brown seaweed (Iodine).
  • Gelatin from fresh hide or bone (Gelatin).
  • Barite (heavy spar): a white, pink or grey mineral, startlingly heavy for its size (heft it against a stone of the same size: it is nearly twice as heavy), soft enough to scratch with a knife, often in veins with lead ores (Rocks and Minerals).
  • Cotton or linen rags for the base paper (Paper).

Making the emulsions

All work after the silver is added is under deep red light for bromide, amber for chloride. Keep notes of every weight, temperature and minute.

Slow chloride emulsion (gaslight paper)

  1. Soak 15 g gelatin in 150 ml water for 20 minutes, melt at 40 °C, and dissolve 4 g salt in it.
  2. Dissolve 10 g silver nitrate in 50 ml water at 40 °C.
  3. Pour the silver into the gelatin in a thin stream over about 2 minutes, stirring hard. It turns a bluish, translucent milk.
  4. Do not ripen. Pour at once into a dish and chill until set (an hour on cold stone).

This emulsion is slow enough to handle by a weak candle or amber light a couple of metres away. It gives crisp, contrasty contact prints from ordinary negatives.

Bromide paper emulsion (1 litre)

Enough for about 4–5 square metres of paper.

  1. Solution A: 300 ml water, 12 g gelatin, 26 g potassium bromide, 0.6 g potassium iodide, at 55 °C.
  2. Solution B: 30 g silver nitrate in 300 ml water at 55 °C.
  3. Add B to A over 5 minutes with steady stirring.
  4. Ripen at 55 °C: 10–15 minutes for a contrasty paper, 30 minutes for a softer, faster one.
  5. Stir in 40 g gelatin that has soaked in cold water, let it dissolve, then chill to set.

Fast plate emulsion (ammonia method)

Several times faster than the plain "boiled" emulsion of Photography.

  1. Solution A: 8.5 g potassium bromide, 0.3 g potassium iodide and 3 g gelatin in 100 ml water at 40 °C.
  2. Solution B: dissolve 10 g silver nitrate in 50 ml water. Add strong ammonia water drop by drop, swirling. A brown cloud forms, then dissolves. Stop the moment the liquid turns clear again. Make up to 100 ml. Use it within minutes (see Dangers).
  3. Pour B into A over 5 minutes, stirring.
  4. Digest at 40 °C for 30–45 minutes.
  5. Add 15 g soaked gelatin, dissolve, chill to set.

Washing and finishing

The set jelly holds potassium nitrate and the extra bromide. Left in, they crystallise on drying, slow the emulsion and spoil the surface.

  1. Noodle it. Press the cold jelly through coarse canvas, or a plate pierced with 3 mm holes, into a jar of cold water. It falls as thin threads.
  2. Wash in 5–6 changes of water at below 12 °C over 2–3 hours, letting each drain through a cloth. In warm weather, wash with ice or well water, or the noodles swell and dissolve.
  3. Drain for half an hour.
  4. After-ripen: melt and hold at 45–50 °C for 20–60 minutes. Find the best time by test (below): take a spoonful every 15 minutes, coat a small test plate from each, and label them.
  5. Finish: at 38–40 °C stir in, for every litre, 20–30 ml alcohol (to help it flow evenly), 5 ml of 5 % chrome alum solution added slowly (to harden the layer so it does not soften in warm developer), and a few drops of carbolic acid or thymol in alcohol to stop bacteria.
  6. Strain through two layers of fine cloth or a pad of washed cotton wool into the coating jug.

A finished emulsion can be set, kept in a closed jar in a cool dark place for a few days, and remelted. It slowly gains fog, so coat within a week.

1. Mix Silver nitrate poured slowly into warm gelatin and bromide silver nitrate 2. Ripen Held in a water bath, 40–55 °C, 10–60 min: the crystals grow 40–55 °C 3. Set and noodle Chilled jelly pressed through canvas into cold water canvas 4. Wash 5–6 changes of water below 12 °C over 2–3 hours fresh cold water drain 5. After-ripen Melted and held at 45–50 °C, 20–60 min: speed rises 45–50 °C 6. Finish and strain Alcohol, hardener, preservative; strained into the coating jug cloth coating jug
Fig. 1 Making a gelatin emulsion, in six steps under the safelight: silver nitrate poured into warm gelatin and bromide; ripened in a water bath; set and pressed through canvas into noodles; washed in cold water; melted and after-ripened; finished and strained into the coating jug.

Gelatin dry plates

Glass

Cut plates from thin, flat window glass, 1.5–2 mm thick, to standard sizes such as 9 × 12 cm or 13 × 18 cm so they fit every camera and holder (Window Glass). Take the sharp edges off on a stone. Clean with lye and chalk, rinse in distilled water, and sub them with a thin coat of 1 % gelatin and a trace of chrome alum so the emulsion grips (Photography). Dry in racks.

The levelling slab

An emulsion poured on a tilted plate runs thin at one side. A levelling slab sets it level and chills it so it gels in place.

  1. Take a thick slab of plate glass, marble or slate, about 60 × 40 cm.
  2. Stand it on three levelling screws (two at one end, one at the other: three points never rock). Wooden screws in a hardwood frame are fine.
  3. Level it both ways with a spirit level.
  4. Underneath, fit a shallow tray of cold water or ice, so the top stays at 10–15 °C.

Coating by hand

  1. Warm the plate slightly to room temperature; hold it flat on the fingertips of one hand or on a small sucker.
  2. Pour 5 ml of emulsion at 35–40 °C per 9 × 12 cm into the middle of the plate (about 0.45 ml per 10 cm²).
  3. Guide it to the corners with a bent glass rod, tilting the plate a little, until the whole surface is covered. Drain nothing off; the amount sets the thickness.
  4. Lay it on the slab. It sets in 2–5 minutes.

The plate drying cupboard

Slow or uneven drying gives marks, fog and soft emulsion. Plates need clean, moving air at 15–25 °C in total darkness.

  1. Build a tall box of boards with tight joints, painted black inside, with a door sealed by felt strips.
  2. Light traps at top and bottom: zig-zag passages of three or four black baffles, through which air moves but light cannot.
  3. Cover the lower inlet with two layers of fine cloth to filter dust.
  4. Draw air through with a small fan, or by the gentle chimney draught of a warm pipe at the top (never a flame inside).
  5. Inside, grooved racks hold the plates on edge, 2 cm apart.

Plates dry in 6–24 hours. A dry plate looks matt and even, and no longer feels cool and tacky at the corners.

Coating by machine (outline)

From 1880 plates were coated by machine. A belt carries clean plates one after another beneath a warmed trough whose lip lays down a smooth band of emulsion, then over a long chilled table where it sets, and onto racks for the drying room. One machine and two workers coat thousands of plates a day. It is built only when demand is steady.

Paper

The base paper

Use a strong, smooth, well-sized rag paper that will survive an hour wet (Paper). Two common weights: single weight, about 130–150 g/m² (a little heavier than writing paper), and double weight, about 230–250 g/m², for prints that must lie flat.

It must be clean. One speck of iron or copper becomes a black spot or a white halo in every print. Test it: lay a sheet in a weak solution of potassium ferrocyanide with a few drops of acid (Prussian Blue and the Prussiates). Blue dots are iron; reject that batch or wash the pulp more and use clean beaters.

Baryta paper

Most good papers carry a thin coat of barium sulfate ("baryta", "blanc fixe") in gelatin under the emulsion. It makes the paper brilliantly white, gives a smooth surface, stops the emulsion soaking into the fibres, and shields the emulsion from impurities in the paper.

Making barium sulfate from barite.

  1. Grind barite fine and mix with a quarter of its weight of powdered charcoal.
  2. Heat in a covered fireclay crucible at bright red to orange heat, about 1,000 °C, for 1–2 hours (The Kiln). The grey lump is barium sulfide ("black ash").
  3. Outdoors, leach it with hot water. The solution smells of rotten eggs.
  4. Stir in a solution of sodium sulfate (Glauber's salt; roughly one and a half times the barite's weight of the crystals) until no more white powder falls. That powder is pure barium sulfate.
  5. Wash it many times by settling and pouring off. Test the washings with a bright silver coin: any blackening means sulfide is still there, and sulfide fogs every emulsion it touches. Keep washing until the coin stays bright.

Coating. Mix 100 g barium sulfate (as wet paste), 10–12 g gelatin and 100 ml water with a pinch of chrome alum at 40 °C. Coat it on the paper with the coating trough below, dry, and give a second coat. For glossy paper, press the dry baryta paper between polished metal rollers (calendering) or rub it with a smooth agate or glass burnisher; for matt, leave it.

The coating trough

A coating trough lays down a film of exactly the same thickness all over the sheet.

Side view, cut through End view draw in one stroke, 3–5 s Glass blade ground straight Gap 0.2–0.3 mm for paper Warm emulsion 38–40 °C Even coat left behind Paper, taped flat Levelled glass table Shim on the rail thicker shim, thicker coat Blade, face on paper width + 2 cm Rail Gap above paper Paper Finished bromide paper, layers enlarged Emulsion silver bromide in gelatin Baryta barium sulfate in gelatin Rag paper base about 0.2 mm
Fig. 2 The hand coating trough, cut through. A glass or enamelled trough rides on two runners along rails either side of a flat glass table; the paper lies on the table beneath it. Warm emulsion flows out under the straight front blade, which is held a fixed gap above the paper by shims under its ends, so every part of the sheet gets the same thickness. The end view shows how shims under the runners set the gap. Below: the layers of finished bromide paper.
  1. The table. A sheet of thick plate glass, 40 × 60 cm, on the levelling stand, with a straight strip of wood glued along each long edge as a rail.
  2. The trough. Make a V-shaped trough, 3 cm deep, as long as the paper is wide plus 2 cm, from glass strips cemented with wax, or from hardwood soaked in hot paraffin wax and varnished. Every surface the emulsion touches must be glass, glazed, enamelled or well waxed.
  3. The blade. The trough's front lip is a straight glass strip, ground true on a flat plate with fine emery (Abrasives and Grinding Stones). Its bottom edge sits 0.2–0.3 mm above the paper for print paper, 0.4–0.5 mm for plates or film. Set the gap with shims of thin brass or card under the trough's two end runners, which ride on the rails.
  4. Coat. Wet the table, lay the paper face up so it clings flat, and tape the edges. Set the trough at the near end, fill it with emulsion at 38–40 °C, and draw it to the far end in one steady stroke of 3–5 seconds. Do not stop halfway: a stop leaves a line.
  5. Set and dry. Lift the sheet onto the cold slab for 5 minutes, then hang it by clips in the drying cupboard.

Coating paper by machine (outline)

A roll of baryta paper runs under a roller that dips its face into a trough of emulsion kept at 35–40 °C by a water jacket. The web passes a chill box at about 10 °C where the gelatin sets, then hangs in long loops on rods through a drying tunnel of filtered air at 25–35 °C, and is wound up, cut and packed, all in darkness. The same machine with a slot hopper coats film (Photographic Film Base).

Testing speed and contrast

Every batch must be tested before it is used, and its numbers written on the box.

The sensitometer

  1. A standard light. A lamp that is always the same: an electric lamp run from a steady battery, or an oil lamp with a fixed wick height, burning behind a fixed opening, at a fixed distance (1 metre is easy). A lamp and its distance never change once chosen.
  2. A step tablet. A strip of glass with 12 steps, each passing about half the light of the one before. Make it photographically: expose a slow plate in strips for 1, 2, 4, 8 … seconds and develop it, or build it of layers of thin tissue as in Platinum, Salt and Iron-Salt Prints.
  3. A sliding shutter or lens cap, and a clock.
  4. Clamp the test strip of plate or paper behind the tablet, expose for a fixed time (for example 10 seconds), then develop in standard developer for a standard time at 20 °C, stop, fix and wash.

Reading it.

  • Speed: count the steps that show any tone. A batch that shows two more steps than last time is four times faster (each step is a doubling).
  • Contrast: count the steps from the first faint tone to full black. For paper: about 3 steps is a hard paper, 4 normal, 5–6 soft. Plates for the camera cover far more, 7–10 steps.
  • Fog: develop an unexposed piece beside a piece fixed without developing. Paper should look identical; a plate may be faintly grey but not more.

Plotting the density of each step against the step number gives the characteristic curve that Hurter and Driffield introduced in 1890. Its slope is the contrast and its position is the speed.

Grades. Make a contrasty batch (short ripening) and a soft one (long ripening). Mixing them in different proportions before coating gives every grade in between. Label the boxes soft, normal, hard.

Cutting, packing and keeping

Cut paper and plates under the safelight with a guillotine. Pack paper face to face and plates face to face in pairs, separated at the edges by card strips, in black paper inside a closed box. Keep away from fumes: coal gas, fresh paint, turpentine, ammonia and rubber (it gives off sulfur) all fog emulsions. Store cool and dry; paper keeps about a year, plates longer.

1 2 3 4 5 6 7 8 9 10 11 12 more lightless light (each step half the one before) Good 4 steps of tone: normal Fogged no clean white; blacks dull Hard white to black in 2–3 steps Soft 6 steps of tone Count the steps that show tone between full black and clean white. Two more steps of tone than last batch = softer; the whole pattern moved two steps to the right = four times faster.
Fig. 3 The sensitometer test strip read three ways. A good batch shows tone on most steps and clean white at the end. A fogged batch is grey all over. A hard batch jumps from white to black in three steps; a soft batch takes six.

How to tell it worked

  • Clean whites: an unexposed sheet, developed and fixed, matches one that was only fixed.
  • Even coating: a fully exposed and developed sheet is an even black with no streaks, bands or bare corners.
  • Matching batches: the sensitometer strip of each new batch matches the label within one step.
  • Grip: the emulsion stays on through developer, fixer and an hour's wash without frilling at the edges.

Note Troubleshooting. Grey fog everywhere → too much ripening, too warm, free silver (not enough bromide), a safelight leak, sulfide in the baryta, or a fumed storage box. Very slow → too little ripening, or "dead" gelatin; try another lot. Crystals or a powdery bloom on the dry surface → not washed enough. Black spots → iron or copper in the paper, or dust; white spots → dust or air bubbles; strain the emulsion and let bubbles rise before coating. Streaks across paper → the trough stopped or jerked, or the emulsion was too cool and began setting. Emulsion frills off the plate edges → no sub, too little hardener, or processing baths warmer than 22 °C. Soft, sticky layer days after coating → drying too slow or too humid; improve the air flow.

Dangers

Danger Never keep ammonia-silver solution. Silver nitrate dissolved in ammonia, left standing, slowly forms black "fulminating silver", which explodes when touched, even wet. Make it only in the amount needed, use it within minutes, and at once pour any left over into a large volume of salt water to throw down harmless silver chloride. Clean the vessel the same day.

Danger Silver nitrate blackens skin, burns and can blind. Wear eye protection; rinse a splash in the eye with clean water for 15 minutes (Silver Nitrate and Silver Salts).

  • Barium compounds except the sulfate are poisonous: barium sulfide and any barium chloride must never be swallowed or left where children or animals can reach them. The black ash and its leaching give hydrogen sulfide, which smells of rotten eggs at first, then deadens the sense of smell before it kills. Work outdoors, upwind, and never in a pit or shed.
  • Chrome alum and carbolic acid irritate skin; wear gloves.
  • Darkrooms and coating rooms need fresh air, especially with alcohol and ammonia fumes. No flames in a room full of alcohol vapour.

What this unlocks

A steady supply of tested plates and paper makes photography a public service: medical X-Rays, Microfilm and Document Storage libraries, astronomical plates, the documents of Copying Documents and Xerography and Blueprints and Cyanotypes, the separations of Colour Photography and the halftone plates of Printing. The same coating skills, with the emulsion on a plastic web, make film for Cinema: Film Cameras and Projectors and roll cameras (Photographic Film Base). Exact, even thin layers are also the first step towards photoresists in Making Microchips.

How it was first done

Richard Leach Maddox, an English doctor, published the idea of silver bromide in gelatin in 1871. Richard Kennett sold dried gelatin emulsion in 1873, and in 1878 Charles Bennett found that keeping the emulsion warm for days made it far faster, which began the age of the snapshot. George Eastman, then a bank clerk in Rochester, New York, patented a plate-coating machine in 1880 and built his company on it. Josef Maria Eder and Giuseppe Pizzighelli worked out developed silver chloride gelatin papers in 1881, and bromide paper for enlarging became common in the 1880s. Baryta-coated papers came into use in the 1880s and 1890s. Ferdinand Hurter and Vero Charles Driffield, two amateur photographers working in the chemical industry, published their measurements of plate speed and the characteristic curve in 1890. Leo Baekeland brought out the gaslight paper Velox in 1893 and sold it to Eastman in 1899; he later invented Bakelite (Resins: Phenolic, Polyester and Epoxy). In 1925 Samuel Sheppard at Kodak traced the mystery of "good" and "bad" gelatin to traces of sulfur compounds (the story goes, from mustard seed in the cattle's feed), and emulsion makers began adding measured sulfur instead.

Source: content/entries/chemistry/photographic-paper.md