◆ Rebuild

Part 8 · Chemistry

Glues and Adhesives

Boil skin scraps and bones into hide glue, fish skins and swim bladders into fish glue, sour milk into waterproof casein glue, and flour into paste — and know which to use for wood, paper, leather or a wet place. Glue lets you build things that nails and pegs cannot.

Difficulty
●●●●●
Time
Starch paste in 15 minutes; casein glue in a day; hide glue in 2–3 days of soaking and cooking, plus a week to dry
Steps from zero
9 prerequisites →

You need first

Tar, Pitch and GlueHides and Leather

This unlocks

Plywood, Veneer and BoardsGelatinMatchesViolins, Guitars and HarpsBookbinding
The full path from nothing — 9 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Hunting and Trapping
  6. Charcoal
  7. Pottery
  8. Hides and Leather
  9. Tar, Pitch and Glue
  10. Glues and Adhesives

Do them roughly in this order. See it on the tech tree →

Why it matters

A glued joint spreads the load over the whole surface instead of a few pegs or nails, and it does not split the wood. Glue lets you join thin pieces that would crack under a nail, build up thick timbers from thin boards, lay veneers, make composite bows from wood, horn and sinew, bind books, hang Paper on walls, and stick labels on medicine jars. It is also a raw material: glue stiffens and seals paper and cloth (sizing), binds paint and the chalk gesso under it, and holds abrasive grit onto cloth or paper (Abrasives and Grinding Stones).

You already have one glue: the pitch and resin glue of Tar, Pitch and Glue, which sets as it cools and is waterproof. This chapter adds the glues made from animals and plants — stronger, cleaner, and right for wood, paper and leather — and tells you which to use when.

How it works

A glue has to do three things:

  1. Wet both surfaces — flow into every pore and scratch while liquid.
  2. Set — turn solid, by cooling (pitch, hot hide glue), by drying (starch, gum, hide glue), or by a chemical change (casein with lime).
  3. Hold — the solid glue must be strong itself and must cling to both surfaces.

Animal glues (hide, bone, fish) are collagen — the protein of skin, tendon and bone — broken down by long, gentle heating in water into gelatin. Warm gelatin is a runny liquid; as it cools it turns to jelly, and as it dries it becomes a hard, tough, amber solid. It grips wood extremely well: a good hide glue joint is stronger than the wood around it. But water and heat soften it again — a weakness, and also a strength, because a joint can be taken apart with steam and repaired.

Casein glue is milk protein. Lime turns the curd into a glue that sets by chemical reaction as well as drying, and becomes water-resistant.

Starch paste is flour or starch cooked in water until the grains burst and turn into a clear jelly. Weak, but cheap, clean and perfect for paper.

Two rules apply to every glue:

  • Thin glue lines are strong; thick ones are weak. Surfaces must fit closely; glue is not a filler. Press the joint tight.
  • Clean, fresh surfaces. Grease, dust, old glue and a shiny planed or sanded skin all stop glue from wetting. Scrape or plane surfaces just before gluing.

What you need

Glue Raw material Other things Best for
Hide glue Rawhide scraps, trimmings, ears, feet, rabbit skins Slaked lime or ash lye, big pot, cloth Wood joints, furniture, musical instruments, veneers, sizing, gesso
Bone glue Fresh bones As above; acid optional Rough woodwork, sizing
Fish glue Fish skins, heads, swim bladders Pot, cloth Fine wood and leather work, gilding, fining beer
Casein glue Skimmed milk Vinegar, slaked lime Outdoor and damp-place woodwork, laminated beams
Starch paste Wheat or rye flour, rice, potatoes Water, pot Paper, books, labels, wallpaper
Resin and pitch Pine resin, birch tar Charcoal powder, beeswax Hafting tools, waterproof seals — see Tar, Pitch and Glue
Shellac and sealing wax Lac, pine resin Fire Glass and metal to wood, sealing letters and jars

You also need a glue pot: a small pot set inside a larger pot of hot water (a double boiler), so the glue never gets hotter than the water. And clamps — see "Clamping" below.

Where to find it

  • Hide scraps — every Hides and Leather job leaves trimmings, edges, ears, and the thin flesh layer scraped off hides. Rabbit and other small-animal skins make an especially fine glue. Rawhide dried in strips keeps for years.
  • Bones — from every butchered animal (Keeping Animals, Hunting and Trapping). Fresh bones give the most glue; old dry bones much less.
  • Fish — skins, heads, fins and especially the swim bladder, a silvery, balloon-like bag along the backbone of most bony fish. The best come from sturgeon, cod, hake and catfish.
  • Milk — skimmed milk, from cows, goats, sheep or any dairy animal. See Dairy and Cheese.
  • Starch — wheat, rye or rice flour (Grain, Flour and Bread), or starch washed out of grated potatoes or cassava: grate them into water, strain off the pulp, let the white starch settle, pour off the water and dry it.
  • Resin, tar and lac — see Tar, Pitch and Glue and Pigments, Paints and Varnish.

Method 1: Hide glue

1. Limescraps in lime water1–3 weeks 2. Washmany changes of water,a splash of vinegar 3. Cook gently60–80 °C, 3–6 hourssteaming, never boiling 4. Strain and setthrough cloth into trays;jelly overnight 5. Slice and dryon nets, cool and airy,1–2 weeks Repeat steps 3–4 with fresh water for a second and third run
Fig. 1 Making hide glue. Clean scraps are soaked in lime water, washed, and cooked gently below boiling. The liquor is strained and drawn off, set to a jelly in trays, sliced, and dried on nets into hard sheets.
  1. Collect and clean. Gather 5–10 kg of fresh or dried rawhide scraps. Cut them into pieces about the size of a hand or smaller. Scrape off fat and meat.
  2. Lime them. Soak the scraps in lime water — about 1 kg of slaked lime (Lime) per 20 litres of water — for 1–3 weeks, stirring now and then. Lime loosens hair, dissolves blood and fat, and makes the collagen swell so that it gives up its glue easily. (Wood-ash lye at about the strength used for Soap, diluted with three times its volume of water, works more slowly.) Dried scraps soak faster if broken up first.
  3. Wash out the lime. Rinse the swollen scraps in many changes of clean water over a day or two, until the water no longer feels slippery. A last soak with a splash of vinegar per bucket neutralises the rest. Lime left in makes a weak, dark glue.
  4. Cook gently. Put the scraps in a large pot, just cover them with clean water, and heat to 60–80 °C — steaming, too hot to keep a finger in, but never boiling. Boiling breaks the gelatin into short pieces that make weak glue. Keep it there 3–6 hours, stirring now and then.
  5. Draw off the first run. Strain the liquor through a cloth into a clean pot. This first run makes the best glue.
  6. Repeat. Cover the scraps with fresh water and cook again, slightly hotter and longer, for a second and third run of lower quality. Keep the runs separate.
  7. Concentrate. Heat each run gently, uncovered, below boiling, until a drop placed on a cold stone sets to a firm jelly within a minute.
  8. Set and slice. Pour into shallow, wet trays 2–3 cm deep. Leave overnight in a cool place. Cut the firm jelly into thin slices (1 cm) with a wetted wire or knife.
  9. Dry. Lay the slices on nets or racks of string in a cool, airy, shaded place, out of flies. They dry in one to two weeks into hard, glassy, amber sheets. Wet weather or warmth makes the jelly go mouldy and liquefy before it dries — dry in cool, breezy weather.

Yield: roughly 1 kg of dry glue from 5–8 kg of fresh, wet scraps, or from 2–3 kg of dry rawhide.

Using hide glue

  1. Break the dry glue into small pieces and soak them overnight in cold water: about 1 part glue to 1½–2 parts water by weight. They swell into a soft jelly.
  2. Heat in the glue pot to about 60 °C — hot to the hand, never boiling. It should run off a brush in a thin, continuous stream like warm honey, and break into drops at the end. Too thick: add hot water. Too thin: heat uncovered a little.
  3. Warm the pieces to be glued (on a warm hearth, not hot) — cold wood chills the glue before it can soak in.
  4. Brush glue on both surfaces, press them together, and rub the joint back and forth a little to squeeze out air and excess glue. Clamp within a minute or two, before it gels.
  5. Leave 12–24 hours before working the piece.

Tip The rubbed joint. Two planed edges of a board can be glued without any clamp at all: brush both, put them together, and slide one back and forth a few times until you feel it grab. Atmospheric pressure and the gelling glue hold it. Leave it standing for a day. This is how wide tabletops were joined for centuries.

Size and gesso

Size is hide glue thinned with about 10–15 times its weight of water. Brushed on paper, it stops ink from spreading (Paper); on cloth or canvas, it stiffens and seals it before painting. Gesso is size with chalk or gypsum stirred in until it is like thick cream — the white ground under paintings and gilding (Pigments, Paints and Varnish).

Method 2: Bone glue

  1. Break fresh bones with a hammer into walnut-sized pieces.
  2. Boil them in water for 1–2 hours to free the fat; skim off the fat as it rises, and keep it for Soap or candles. (Here boiling is fine — it is the glue you will extract later that must not boil.)
  3. Pour off the fat water. Cover the bones with fresh water and cook at just below boiling for 6–12 hours, topping up with hot water.
  4. Strain off the liquor and concentrate it as for hide glue. Repeat with fresh water.

Bone glue is darker and weaker than hide glue but perfectly good for rough work and sizing. For a much better yield, soak the broken bones for 1–2 weeks in dilute Hydrochloric Acid — about one part strong acid to ten parts water — until they are soft and rubbery: the acid dissolves the mineral and leaves the collagen (ossein), which you then lime and cook as for hide glue. The acid liquor holds the phosphorus of the bones — a fertiliser (Chemical Fertilisers).

The leftover bones can be burnt for bone ash or bone black (Pigments, Paints and Varnish) or ground for fertiliser (Compost and Manure).

Method 3: Fish glue

  1. Swim bladders (isinglass): wash them, slit them open, scrape off the outer membrane and blood, and dry them flat in the sun. To use, cut a small piece into shreds, soak it overnight in a little water, then warm it gently in a glue pot until it melts into a thick, clear syrup. It is the clearest and one of the strongest glues there is — for fine woodwork, repairing glass and porcelain, and fining beer and wine (a pinch stirred in makes cloudiness settle — see Beer, Wine and Cider).
  2. Skins and heads: rinse well in fresh water, soak a day in cold water to remove salt and blood, then simmer gently below boiling for 4–8 hours. Strain and boil down slowly to a thick syrup.

Fish glue stays liquid at room temperature (no glue pot needed), gives you more time to fit a joint, and sticks to leather, parchment and metal leaf. It smells — store it with a few drops of vinegar or clove oil, in a closed jar.

Method 4: Casein glue

This is the most water-resistant glue in the chapter that you can make without chemistry beyond lime. It glued wooden aircraft in the First World War and the first laminated timber beams.

Make the casein

  1. Warm 10 litres of skimmed milk to about 35–40 °C (blood warm). Stir in vinegar, about a cupful at a time (roughly 0.5 litre in all), until the milk separates into white curds and clear, greenish whey.
  2. Strain through a cloth. Wash the curds in warm water three or four times, squeezing well each time, to remove whey and any fat. Fat ruins casein glue.
  3. Use the wet curd at once, or crumble it and dry it in the sun or a cool oven on a cloth. Dry casein keeps for years. Expect about 300 g of dry casein from 10 litres.

Mix the glue

  1. From dry casein: soak 100 g of ground casein in 250 ml of water for half an hour.
  2. In another pot, stir 25 g of slaked lime into 100 ml of water.
  3. Pour the lime into the casein, stirring hard. It will thicken, then thin, and become smooth and creamy in 10–15 minutes. Let it stand 15 minutes more.
  4. From fresh curd: knead curd squeezed fairly dry with about one fifth of its volume of lime putty until it turns smooth and sticky.
  5. Use within 4–6 hours. It then sets solid in the pot, so mix only what you need.

Brush on both surfaces and clamp tightly for 6–12 hours at room temperature (above 10 °C). Full strength comes after several days. Casein stains some woods dark (oak, for example), because lime reacts with their tannin.

Method 5: Starch paste

  1. Stir 1 part wheat flour or starch into 2 parts cold water to a smooth cream with no lumps.
  2. Pour this into 4–6 parts boiling water, stirring hard. Keep stirring over gentle heat for 5–10 minutes until it turns from milky white to translucent and thick, like a soft jelly.
  3. Cool it. Push it through a cloth or sieve to remove lumps. It keeps a few days; a pinch of alum (Dyes and Mordants) or a few drops of clove oil makes it keep longer.

Use thin for paper, labels and bookbinding (Bookbinding); thicker, with rye flour, for wallpaper and cloth. Rice paste is the clearest and finest — the paper conservator's paste of East Asia.

Dextrin — "British gum" — is starch roasted dry on a tray at 150–200 °C until it turns pale yellow to tan, about an hour. It then dissolves in cold water into a thick gum, perfect for envelopes, labels and stamps.

Resin, pitch and sealing wax

The pitch glues of Tar, Pitch and Glue remain the best waterproof glue for hafting tools and sealing seams. Two refinements:

  • Shellac cement: melted lac (Pigments, Paints and Varnish) sticks glass, stone and metal to wood — jewellers and lens-makers (Lenses) hold small work on a stick with it. Heat the parts, dab on, press, let cool. Reheat to release.
  • Sealing wax: melt 4 parts lac, 1 part pine rosin and a little chalk and red ochre, stir, and roll into sticks on a wet stone. Used to seal letters, jars and bottle corks.

Clamping

Glue is only as good as its pressure. Without metal clamps:

Sticktwist, then lock drive Glue line Glue line Veneerbetween flat boards Rope windlasspads stop the rope denting Opposed wedgesbetween fixed blocks Weightsstones on a board
Fig. 2 Clamping without metal tools. A rope twisted tight with a stick (a windlass), a pair of wedges driven against a fixed block, and heavy stones on a flat board all press a joint closed while the glue sets.
  • Rope windlass: loop a doubled rope around the work, put a stick through the loop and twist until tight, then lock the stick against the work.
  • Wedges: fix two blocks to a board or beam; put the work between them and drive a pair of opposed wedges between one block and the work.
  • Weights: stones or bags of sand on a flat board laid over veneers or panels.
  • Binding: wrap the joint tightly with wet rawhide strips or cord; as they dry they shrink and squeeze.
  • Screw clamps made of wood once you can cut screws.

Use pads of scrap wood under ropes and wedges so they do not dent the work, and enough pressure to squeeze a thin bead of glue out along the whole joint.

How to tell it worked

  • Break test: glue two scraps of the same wood end to end or face to face, let them cure a day, and break them over your knee or with a hammer. If the wood tears and leaves fibres stuck to the glue on both sides, the glue is stronger than the wood — good. If the pieces part cleanly along a shiny glue line, the glue (or your joint) failed.
  • Hide glue sheets should be hard, glassy and snap with a sharp crack. A sheet that bends like leather is not dry; a dark, cloudy, smelly one was overheated or went off.
  • Jelly test: a drop of hide or bone glue on a cold stone should gel firmly within a minute.
  • Water test for casein: soak a cured test joint in water for a day. It should still be firm.

Note Troubleshooting. Joint fails cleanly along the glue line → glue too thin or too thick, chilled before clamping, too little pressure, greasy or dusty surfaces, or (for hide glue) overheated or boiled glue. Warm the wood; scrape fresh surfaces; clamp sooner and harder. Hide glue goes mouldy and smells → warm, damp storage. Dry sheets fully; make up only what you will use in a few days; add a little vinegar. Glue jelly will not set → too dilute, or boiled. Concentrate further; next time keep below boiling. Casein glue lumpy → not enough lime, curd not washed, or fat left in. Wash curds well; stir longer. Starch paste lumpy → flour added straight to hot water. Always make a cold cream first. Joint opens in damp weather → hide, fish and starch glues are not waterproof. Use casein, or pitch, for wet places.

Dangers

Danger Anthrax from hides and bones. Hides, hair, wool and bones from animals that died of disease — especially sudden, unexplained deaths with dark blood from the nose or mouth — can carry anthrax spores that survive for decades. Glue works and wool sorters once died of it. Never use skins or bones from animals that died sick. Bury such carcasses deep, away from water and grazing. Wash hands with soap after handling scraps, cover cuts, and do not shake dry hides indoors. See Animal Health and Infectious Diseases.

  • Lime for liming scraps and casein glue burns eyes and skin. Protect your eyes; rinse splashes with water for 15–20 minutes (Lime).
  • Hot glue and molten resin stick to skin and burn deeply. Keep a pot of cold water at hand to plunge a burnt finger into; do not pull off stuck resin.
  • Rotting scraps draw flies and rats. Keep them covered, lime them promptly, and work away from houses and wells.
  • Hydrochloric acid for bone glue — see its own chapter for safe handling.

What this unlocks

Glue opens fine woodworking: Furniture, Musical Instruments, laminated bows (Bow and Arrow), plywood and laminated timber (Plywood, Veneer and Boards) for Roofs, boats and Gliders and Aeroplanes. It binds books and sizes Paper. It holds grit onto cloth to make sandpaper (Abrasives and Grinding Stones) and makes the heads of Matches. Gelatin itself — the purest hide glue (Gelatin) — is used in Photography and cooking. Casein glue led to casein plastic (Early Plastics), and the search for better glues to rubber cements and synthetic resins (Resins: Phenolic, Polyester and Epoxy).

How it was first done

The oldest known glue is birch tar, made by Neanderthals in Europe at least 200,000 years ago (Tar, Pitch and Glue). Animal glue appears in Egypt: wooden furniture from tombs more than 4,000 years old was glued and veneered, and a wall painting in the tomb of Rekhmire at Thebes, from about 1450 BC, shows a glue pot heating over a fire. Greek and Roman carpenters used hide and fish glue; Pliny the Elder (1st century AD) described isinglass. The monk Theophilus, writing in the early 12th century, gave recipes for hide glue and for cheese (casein) glue mixed with lime. The first glue factory is said to have opened in Holland around 1690, and the first British patent for a glue — a fish glue — was granted in 1754. Casein glue was produced industrially from about 1900 and glued Otto Hetzer's laminated timber beams (patented in 1906) and the wooden aircraft of the First World War. Synthetic resin glues began to replace natural glues from the 1930s.

Source: content/entries/chemistry/glues-and-adhesives.md