◆ Rebuild

Part 14 · Electronics and Computing

Piezoelectric Crystals and Ceramics

Crystals and fired ceramics that turn a squeeze into a voltage and a voltage into a movement. Grow Rochelle salt crystals for microphones and pickups; fire barium titanate and lead zirconate titanate like porcelain and "pole" them with high voltage; and make the buzzers, gas-lighter sparkers, ultrasonic cleaners, echo sounders, sensors and fine-motion actuators they make possible.

Difficulty
●●●●●
Time
Two to four weeks to grow a large Rochelle salt crystal; a week of firing trials for first ceramic discs; a day to build each device once you have them
Steps from zero
33 prerequisites →

You need first

Quartz Crystals and Frequency ControlStoneware and Porcelain

This unlocks

—
The full path from nothing — 33 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. The Kiln
  9. Pottery
  10. Charcoal
  11. Abrasives and Grinding Stones
  12. Hides and Leather
  13. Lime
  14. Bricks
  15. Mercury
  16. Lye and Potash
  17. Fermentation
  18. The Wheel and Axle
  19. Glass
  20. Firebrick and Refractories
  21. Bellows
  22. The Lathe
  23. Glazes
  24. Copper Smelting
  25. Laboratory Glassware
  26. Pumps
  27. Stoneware and Porcelain
  28. The Battery
  29. The Vacuum Pump
  30. The Light Bulb
  31. The Vacuum Tube
  32. Amplifiers and Oscillators
  33. Quartz Crystals and Frequency Control
  34. Piezoelectric Crystals and Ceramics

Do them roughly in this order. See it on the tech tree →

Why it matters

Quartz Crystals and Frequency Control showed that quartz gives a tiny voltage when squeezed and moves a tiny amount when given a voltage — enough to hold a radio on frequency, far too little to make a loud sound or a strong push. Other materials do the same a hundred to a thousand times more strongly. With them:

  • A coin-sized disc on a battery makes a piercing buzzer for alarms, clocks and machines (Electric Bells, Buzzers and Alarms).
  • A spring-loaded hammer striking a small ceramic cylinder makes a spark of 10,000 volts or more with no battery — the igniter of gas stoves and lighters.
  • Ceramic rings clamped between steel blocks shake 40,000 times a second and scrub anything in a water tank clean: the ultrasonic cleaner.
  • The same transducer times echoes in water: the echo sounder, and the probes of Ultrasound, CT and MRI.
  • In reverse the ceramic senses sudden force, sound and vibration, and stacked up it is an actuator that moves by millionths of a millimetre.

How it works

Charges locked in a crystal

In some crystals the positive and negative charges of the atoms are not quite centred. Squeeze the crystal and they shift: a voltage appears. Apply a voltage and they shift, changing the crystal's shape. This is piezoelectricity (Quartz Crystals and Frequency Control).

Why ceramics must be poled

Barium titanate and lead zirconate titanate (PZT) are far stronger than quartz but are made as ceramics — grains fired together like porcelain. Each grain holds regions (domains) whose charges point every which way, so a fresh disc does nothing.

You wake it up by poling: warm it, put a strong voltage across it — 1,000–3,000 volts per millimetre of thickness — and let it cool with the voltage still on. The domains swing into line and freeze there. The disc now has a "+" face and a "−" face.

Heat undoes poling. Above its Curie temperature — about 120 °C for barium titanate, 330–370 °C for PZT — the domains scramble again. Keep parts well below half that, and never solder long on a poled disc.

Strengths compared

Material Strength (quartz = 1) Upper limit Notes
Quartz 1 573 °C Very stable; for frequency control
Rochelle salt over 100 Strongest −18 to +24 °C; melts at 55 °C Easy to grow; spoils in damp or very dry air
Barium titanate about 80 120 °C First ceramic; easier to fire
PZT 130–270 330–370 °C The standard since the 1950s

Resonance

Every piezoelectric part rings at a frequency set by its size, like a bell, and moves many times more when driven at it. A PZT plate ringing through its thickness: frequency in megahertz ≈ 2 ÷ thickness in mm. A buzzer disc bending like a drumhead rings at a few thousand cycles a second.

What you need

Item Details
Rochelle salt Wine tartar (Citric and Tartaric Acid), washing soda (Soda Ash and Baking Soda), glass jars, a steady warm cupboard
Barium carbonate From barite (The Vacuum Tube shows how)
Titanium dioxide Titanium white from ilmenite or rutile (Titanium)
Lead oxide Litharge, the yellow oxide skimmed from melted lead (Lead)
Zirconium oxide From zircon sand (Zircon and Zirconium)
Mill, die, press, kiln As for porcelain and ferrite (Stoneware and Porcelain, Transformer Steel, Ferrite and Magnetic Shielding); a kiln to 1,350 °C with covered alumina or fireclay crucibles (The Kiln, Firebrick and Refractories)
Silver For electrodes (Silver Nitrate and Silver Salts)
High voltage 0–5 kV DC, current-limited (Power Supplies and Regulators, The Induction Coil with a rectifier)
Oil bath Clean mineral or transformer oil (Petroleum and Refining) in a steel pot on a heater, with a The Thermometer
Testing Meter, oscillator (Amplifiers and Oscillators), earphone or oscilloscope
Brass sheet 0.2–0.3 mm (Zinc and Brass)

Where to find it

Wine tartar is the crust inside wine barrels (Citric and Tartaric Acid); soda from desert soda lakes or made from salt (Soda Ash and Baking Soda). Barite is remarkably heavy pale crystals in veins with galena (X-Rays). Rutile, ilmenite and zircon are heavy grains in black beach and river sands (Titanium, Zircon and Zirconium). Galena, for lead, is heavy grey cubes (Lead).

Rochelle salt crystals

Rochelle salt (potassium sodium tartrate) is the easiest strong piezoelectric to make. Quartz Crystals and Frequency Control gives the recipe from cream of tartar and soda; here is how to grow it big.

  1. Saturate clean rain or distilled water with purified Rochelle salt at 35–40 °C — roughly 1 kg per litre — and filter it hot into a clean jar. Dust becomes a crop of tiny crystals.
  2. Hang a seed, a small clear crystal from an earlier batch, on a fine thread once the solution has cooled a degree or two below saturation. If it dissolves, the liquid is too warm; if it grows a fur of small crystals, too cold.
  3. Cool about half a degree a day: pack the jar in straw or stand it in a big tub of water, covered against dust.
  4. Harvest after 2–4 weeks: a clear, sharp-faced crystal 5–10 cm long.

Cutting: Rochelle salt dissolves in water, so saw it with a wet cotton thread drawn back and forth, and smooth faces on a damp cloth over glass. Cut plates 0.5–1 mm thick in different directions, fix foil to both faces with a touch of wax, connect an earphone and tap: keep the direction that clicks loudest (the best bending plates lie across the crystal's long axis with edges at 45° to the other two). Electrodes: fine graphite in thin varnish, or tinfoil.

Protect it: above about 80 % humidity it dissolves; below about 30 % it dries white and crumbly. Dip finished parts in molten wax or lacquer, and keep them below 45 °C.

Microphone, pickup and earphone

Glue two plates face to face so one stretches while the other shrinks, wired so their voltages add. This bimorph bends strongly:

  • Crystal microphone: a bimorph 2–3 cm square held at three corners, the fourth linked to a paper or foil diaphragm 3–5 cm across. Tens of millivolts, into an amplifier with a very high input resistance — a valve grid with a 1–5 megohm grid resistor (The Vacuum Tube, Amplifiers and Oscillators).
  • Crystal pickup: the needle holder twists a bimorph strip, giving up to a volt (Recording Sound).
  • Crystal earphone: a bimorph driving a small cone; it needs almost no current, ideal for a crystal set (Radio).

Ceramic piezoelectrics

Barium titanate

  1. Weigh 247 g barium carbonate to 100 g titanium dioxide (equal numbers of barium and titanium atoms). Both pure: tenths of a per cent of iron or silica spoil it.
  2. Mill wet in a porcelain ball mill 12–24 hours (Stoneware and Porcelain); dry.
  3. Calcine in a covered crucible at 1,100–1,200 °C for 2–4 hours. Carbon dioxide leaves; the powder turns pale cream.
  4. Mill again very fine, add 1–2 % dextrin or wax as binder, dry and sieve into granules.
  5. Press discs at 1–2 tonnes per square centimetre, 20 % oversize for shrinkage.
  6. Sinter at 1,300–1,350 °C for 2 hours in air, heating slowly (2 °C a minute) to 500 °C to burn out the binder.

A good disc is ivory, hard, rings when tapped, and does not stick to a damp tongue (no open pores).

Lead zirconate titanate (PZT)

  1. Weigh lead oxide 223 parts, zirconium oxide 64, titanium dioxide 38, plus 1–2 % extra lead oxide for what evaporates. About 1 % niobium oxide makes it "soft" — sensitive, for sensors and buzzers; a little iron or manganese oxide makes it "hard" — for high-power transducers and igniters.
  2. Mill, calcine at 800–900 °C, mill again, bind and press as above.
  3. Sinter at 1,200–1,280 °C for 1–2 hours in a closed crucible, the parts bedded in packing powder of the same mix with extra lead zirconate. This keeps a lead-rich atmosphere; without it the parts lose lead and come out weak and porous.

Electrodes and poling

Lap sintered parts flat and to thickness with fine abrasive on glass (Abrasives and Grinding Stones, Gem Cutting and Lapidary). For silver electrodes, precipitate fine silver powder by stirring clean copper into silver nitrate solution (Silver Nitrate and Silver Salts); mix 7 parts silver with 1 part low-melting lead–borax glass powder (Enamel on Metal) and pine oil or turpentine to a paint; brush it on both faces and fire at 600–750 °C for 10–20 minutes. The silver bonds through the glass and takes solder.

half a wavelength:55–65 mm at 40 kHz Steel back mass PZT rings poled opposite ways Aluminium front mass bolt squeezes rings, 25–35 MPa hot electrode Movement along the stack still point (mount here)ends move most,in opposite ways Poling heat, apply voltage, cool with the voltage on 10–100 MΩ HV 2–3 kV per mm Mineral oil 120–150 °C for PZT Heater disc
Fig. 1 Left: the Langevin ultrasonic transducer. Two ceramic rings, poled in opposite directions with an electrode between them, are squeezed between a steel back mass and an aluminium front mass by a central bolt. The whole stack is half a wavelength long. Right: poling. The silvered ceramic sits between electrodes in hot oil while a high voltage is applied, then cools with the voltage still on.

Poling:

  1. Clip the clean, dry, electroded parts in a rack and lower them into clean, dry mineral oil, which stops sparks creeping round the edges.
  2. Heat the oil to 100–120 °C for barium titanate, 120–150 °C for PZT.
  3. Raise the voltage gradually to 1–2 kV per mm of thickness for barium titanate, 2–3 kV per mm for PZT, through a 10–100 megohm resistor so a breakdown cannot burst the disc.
  4. Hold 10–30 minutes, then let the oil cool below 50 °C with the voltage on.
  5. Turn down, short the electrodes together, and mark the positive face.

Discs that crack or short had pores or cracks — a test in itself.

The piezo disc and buzzer

Front cap hole 2–3 mm, tuned air space (Helmholtz) PZT disc 20 mm, 0.2 mm, silvered Brass disc 27 mm, 0.2–0.3 mm feedback lead brass lead Back housing disc held by its rim silver lead no voltageflat voltage one waydishes up reverseddishes down Edge viewceramic tries to shrink or grow;the brass resists, so it bends
Fig. 2 A piezo disc and buzzer, exploded. A thin ceramic disc with silver on both faces is glued to a larger brass disc. When a voltage makes the ceramic shrink, the brass resists and the pair bends like a drumhead. Mounted at its edge in a housing with a small hole, it makes a loud note.

The disc: a PZT disc 20 mm across, 0.2–0.25 mm thick, silvered both faces, glued centred on a brass disc 27 mm across, 0.2–0.3 mm thick with the thinnest layer of epoxy or shellac, pressed hard while it sets; the rough silver touches the brass through the glue, so the brass is the second electrode. For a self-driving buzzer, scratch a 0.5 mm gap to cut a small feedback island off the top silver. Solder leads quickly with a small hot iron and low-melting solder.

When the ceramic tries to shrink across its width the brass refuses, and the pair dishes, like a bimetal strip (Thermostats and Automatic Control). Alternating voltage makes it flex in and out: sound.

The buzzer:

  1. Hold the disc by its rim (its still circle is near the edge) with soft rubber or glue in a short cylinder of wood, plastic or metal.
  2. Close the front with a cap with a 2–3 mm hole. The air behind the cap and in the hole form a Helmholtz resonator — what makes a bottle hoot — tuned to the disc's note; adjust hole and depth for the loudest sound.
  3. Drive it with a square wave at resonance, about 3–5 kHz, at 3–30 V (Amplifiers and Oscillators, Electronic Counters); or self-drive it, the feedback island feeding the base of a transistor whose collector drives the main electrode (Semiconductors and the Transistor), so it needs only a battery.

A good one is ear-piercing at 10 cm (about 85 decibels) on a few milliamps from 9 V. Glued to a guitar body or a door, the same disc is a contact microphone or tap sensor.

The piezo igniter

++−− Button Strong spring button squeezes it Hammer steel, a few grams Catch trips at end of stroke Anvil Two PZT cylinders + ends together Steel frame earth side Centre electrodespark lead, insulated Spark10–20 kV, 3–5 mm gap Burner gas frame and burner both earthed
Fig. 3 The piezo spark igniter in section. Pressing the button compresses a strong spring behind a steel hammer. At the end of the stroke a catch releases the hammer, which strikes an anvil on two small ceramic cylinders. The sudden squeeze makes many thousands of volts between the centre electrode and the frame, which jump the spark gap at the burner.
  1. Ceramic: two hard PZT cylinders about 3 mm across, 6–8 mm long, poled lengthwise, stacked with positive ends together on a brass centre electrode. Their outer ends touch the metal frame (earth); the centre electrode carries the spark lead.
  2. Frame: strong steel or brass, so the blow goes into the ceramic. An anvil sits on top of the stack.
  3. Hammer: a steel slug of a few grams in a guide, pushed by a stiff coil spring (Springs) that the button compresses.
  4. Catch: a small lever holds the hammer back until the button nearly bottoms, then trips it.
  5. Spark lead: insulated wire to a point 3–5 mm from the burner's earthed metal.

Each click gives 10,000–20,000 volts but very little energy — a sting, not a dangerous shock — and lights the gas every time, with no battery, match or flint. A slow squeeze lever on a larger ceramic also works, but the impact type gives a stronger spark from a smaller element.

Ultrasonic transducers

Thickness disc (megahertz). A silvered PZT disc rings at about 2 MHz divided by its thickness in mm: 1 mm thick rings near 2 MHz, 2 mm near 1 MHz. Backed with a damping block and faced with a matching layer it sends short pulses (Ultrasound, CT and MRI). Driven continuously at about 1.7 MHz under 3–5 cm of water, it throws up a mist: the ultrasonic humidifier.

The bolt-clamped transducer (20–40 kHz). Ceramic shaken hard breaks, because it is weak in tension. Paul Langevin's answer (1917) was to clamp it between metal:

  1. Rings: two hard PZT rings, for example 38 mm outside, 15 mm inside, 5 mm thick.
  2. Stack, back to front: steel back mass; copper ring (earth); ring 1; copper electrode with a tag (hot); ring 2 turned the other way round; copper ring (earth); aluminium front mass, flared for a cleaner or tapered into a horn for welding.
  3. Bolt: high-tensile steel through the middle, sleeved so it cannot touch the hot electrode, tightened to squeeze the rings at 25–35 megapascals so they are never pulled apart.
  4. Length: half a wavelength of sound. Sound in steel and aluminium travels about 5 km a second, so a 40 kHz stack is about 55–65 mm, a 20 kHz one about twice that. Make the front mass long, measure the resonance, and turn it shorter on the The Lathe until it rings where you want.

The middle hardly moves; both ends move most. Mount it there with a thin flange, or glue its face to the work. Drive it with a power oscillator at resonance, with a coil in series to cancel the ceramic's capacitance (Power Electronics and Motor Drives).

The ultrasonic cleaner

A stainless steel tank with transducers epoxied or bolted under its floor — about one 50 W transducer per 2–3 litres — in parallel, driven at 40 kHz. Fill with warm water and a little detergent (Detergents and Wetting Agents). The sound tears the water into countless tiny bubbles that collapse violently on every surface — cavitation — scouring cracks no brush can reach: surgical instruments before Sterilising Instruments and Dressings, jewellery, injector parts, laboratory glass, circuit boards. Test: a strip of aluminium foil hung in the bath for a minute comes out peppered with holes.

The echo sounder

Sound travels about 1,500 m a second in water, so each millisecond of echo delay means 0.75 m of depth.

  1. A transducer of 50–200 kHz faces down through the hull or hangs over the side in a streamlined housing.
  2. A pulser dumps a charged capacitor through it for a fraction of a millisecond, a few times a second (Ultrasound, CT and MRI).
  3. The same transducer then listens; a high-gain amplifier boosts the echo.
  4. Flasher display: a neon lamp on an arm spun by a motor once per pulse (Arc Lamps, Neon and Fluorescent Lights). It flashes at "zero" as the pulse leaves and again when the echo returns, against a depth scale round the dial; fish show as faint flashes above the bottom.

It finds channels, anchorages and fish (Fishing, Steamships) and charts harbour bottoms (Maps and Mapmaking).

Sensors and actuators

  • Sensors: a ceramic disc under a small mass is an accelerometer for machine vibration; screwed into an engine, a knock sensor; sealed in rubber, a hydrophone. Charge leaks away, so they sense changing force only — impacts, vibration, sound — never a steady weight (use a strain gauge, Photocells and Sensors). Feed them into a very high input resistance.
  • The piezo actuator: ceramic grows by only about 0.1 %, but precisely and with great force. A stack of 50 discs 0.2 mm thick with electrodes between them, alternately connected, grows about 10 micrometres at 400 V. Such stacks move microscope stages, tune laser mirrors (Lasers), snap fast valves, and in miniature fire printer ink jets (Displays, Printers and Data Storage).

How to tell it worked

  • Rochelle salt: clear, sharp-faced, no white crust; a pencil tap clicks loudly in an earphone.
  • Ceramic: dense, rings when tapped, no tongue stick, no cracks under a lens.
  • Poling: squeezed between finger and thumb with a meter on its most sensitive range, the needle kicks one way on pressing, the other on release. Unpoled gives nothing.
  • Resonance: in series with a resistor across an oscillator, the voltage across the part dips sharply at resonance as you sweep the frequency.
  • Buzzer loud on milliamps; igniter a fat blue spark across 4 mm every click; cleaner passes the foil test; echo sounder agrees with a lead line to a few per cent.

Note Troubleshooting. Rochelle salt grows as a crust of small crystals → too cold, cooled too fast, or dusty. Crystal goes white and powdery → air too dry; seal it in wax. Ceramic porous → under-fired, or lead lost; hotter, or use packing powder. Disc cracks in the kiln → too fast to 500 °C. Disc shorts while poling → cracks, pores or silver on the edge; clean the edge, raise the voltage more slowly. Weak after poling → too cool, voltage too low, or switched off before cooling; repole. Device weakens over time → overheated by soldering, sun or engine; use hard PZT and keep it cool. Transducer dies at high power → bolt loosened or ring cracked.

Dangers

Danger Lead. PZT is more than half lead oxide. Milling, calcining and sintering release lead dust and fume that build up in the body and harm the brain, nerves, kidneys and unborn children (Lead). Mill wet, fire under a hood, wear a mask and gloves with powders, wash before eating, and keep children out.

Danger High voltage and hot oil. The poling supply can kill: current-limit it, interlock the cover, keep one hand away, and short every disc and capacitor before touching (Wiring and Electrical Safety). Oil at 150 °C burns deeply and can catch fire: thermometer always in, never unattended, a lid ready to smother it, no water near.

  • Barium carbonate is poisonous if swallowed (it was used as rat poison). Silver nitrate stains and burns skin (Silver Nitrate and Silver Salts).
  • Do not hold fingers in a running ultrasonic bath; wear ear protection near 20 kHz welders.
  • Keep igniter sparks away from anyone with a heart pacemaker.

What this unlocks

How it was first done

Pierre and Jacques Curie discovered piezoelectricity in Paris in 1880 in quartz, tourmaline, cane sugar and Rochelle salt — first made by the apothecary Pierre Seignette of La Rochelle around 1675. Hunting submarines in 1917–18, Paul Langevin sandwiched quartz between steel plates and sent ultrasonic pulses through the sea; ships' echo sounders followed in the 1920s. Joseph Valasek found in 1920 that Rochelle salt behaves electrically as iron does magnetically — the first ferroelectric — and in the 1930s the Brush Development Company of Cleveland, under Charles Baldwin Sawyer, grew it by the tonne for millions of microphones, earphones and pickups based on Sawyer's 1931 "bimorph". Barium titanate was found to be ferroelectric in the United States, the Soviet Union and Japan in 1943–46; Robert Gray of the Erie Resistor Company showed in 1946–47 that a poled ceramic acts like a crystal, and barium titanate pickups were on sale by 1947. In 1954 Bernard Jaffe, Robert Roth and Samuel Marzullo at the US National Bureau of Standards discovered PZT. Igniters, buzzers and ultrasonic cleaners spread from the 1950s to the 1970s, the buzzers made by the hundred million in Japan.