Part 8 · Chemistry
Waxes: Beeswax, Plant Waxes and Paraffin
Waxes are the soft, water-shedding solids that melt in hot water and set again on cooling. How to clean and bleach beeswax, win carnauba, candelilla and bayberry wax from plants, refine paraffin wax from oil, and use them for polish, candles, seals, casting patterns, batik and waterproof cloth.
- Difficulty
- ●●●●●
- Time
- An afternoon to clean a batch of beeswax; two to four weeks to sun-bleach it; a day to boil out plant wax; an hour to make polish
- Steps from zero
- 18 prerequisites →
This unlocks
—The full path from nothing — 18 steps before this one
- Fire
- Cordage and Rope
- Stone Tools
- Finding and Preparing Clay
- Finding and Identifying Ores
- Beekeeping
- Hunting and Trapping
- Basic Woodworking
- Pottery
- Charcoal
- Hides and Leather
- Fermentation
- Bellows
- Distillation
- Iron (the Bloomery)
- Blacksmithing
- Steel
- Petroleum and Refining
- Waxes: Beeswax, Plant Waxes and Paraffin
Do them roughly in this order. See it on the tech tree →
Why it matters
Wax is the material you reach for when something must shed water, slide, seal, take a fine shape, or burn cleanly. It makes the best candles. It feeds and shines wood, leather and floors. It seals jars, cheeses and letters, waterproofs thread and cloth, and holds the shape of a casting until the metal replaces it (Metal Casting). It resists dye in patterned cloth and insulates wires and coils. Unlike fats and oils, a good wax does not go rancid. A block of beeswax keeps for centuries.
Beekeeping shows how to render wax from comb, and Petroleum and Refining how wax first separates from heavy oil. This chapter covers what comes after: cleaning and bleaching beeswax, the wax-bearing plants for places without bees, refining paraffin properly, and how to make the everyday things that wax is for.
How it works
What a wax is. A true wax such as beeswax or carnauba is a fatty acid joined to one long-chain alcohol; a fat is three fatty acids joined to glycerine (Soap). Wax molecules are long, straight and tightly packed, so wax is harder than fat, melts sharply, repels water and does not turn sour. Paraffin wax is a mixture of long, straight hydrocarbons from oil that behaves the same way. Bayberry and Japan wax are really hard fats that act like wax in candles.
What matters in use: the melting point (a polish or candle must not soften in summer; a modelling wax must soften in the hand); hardness and gloss (carnauba buffs to a high shine but is brittle, beeswax is tough and plastic, so most recipes blend them); and stickiness (beeswax clings, paraffin crumbles, and pine resin makes any wax stickier).
| Wax | Melts at | Character | Main uses |
|---|---|---|---|
| Bayberry | 45–50 °C | Grey-green, fragrant, brittle (really a fat) | Candles blended with beeswax |
| Japan wax (sumac berries) | 50–55 °C | Pale, soft, sticky (really a fat) | Polishes, candles, cosmetics |
| Paraffin | 46–68 °C by grade | White, odourless, crumbly, slippery | Candles, seals, waterproofing, insulation |
| Beeswax | 62–64 °C | Yellow, honey smell, tough, plastic | Everything; the best all-rounder |
| Candelilla | 68–73 °C | Hard, glossy, brownish | Polishes, harder blends |
| Carnauba | 82–86 °C | Hardest, highest gloss, brittle | Floor, shoe and car polish, hardening blends |
| Microcrystalline | 60–90 °C | Flexible, sticky, from oil residue | Cheese coating, blends, casting wax |
What you need
| Item | Use | From |
|---|---|---|
| Double pot, or a pot standing in a pan of water | Melting wax safely | Pots, Pans and Kettles; tin, enamel, aluminium or stainless only |
| Strainers: cheesecloth, felt | Cleaning | Felt, Cotton |
| Moulds: tins, wooden boxes, bread tins | Casting blocks | Tins, Cans, Drums and Tanks |
| Turpentine | Solvent for polish | Distilled from pine resin (Tar, Pitch and Glue, Ether, Acetone and Solvents) |
| Pine resin (rosin) | Stickiness | Tar, Pitch and Glue |
| Thermometer (or the signs given below) | Temperature control | The Thermometer |
| Sulfuric acid, a little | Candelilla | Sulfuric Acid |
Do not melt beeswax in iron, copper, brass or zinc: they stain it brown, green or grey and spoil its quality. Tinned, enamelled, aluminium, stainless steel or glazed pots are all fine.
Where to find it
- Beeswax: comb, cappings and old brood comb (Beekeeping); 0.5–1 kg a year from a strong hive.
- Carnauba palm (Copernicia prunifera): a fan palm 10–15 m tall in groves on seasonally flooded flats of north-east Brazil. In the dry season its stiff fan leaves carry a whitish wax powder that rubs off on the fingers.
- Candelilla (Euphorbia antisyphilitica): clumps of leafless, pencil-thick, grey-green stems 30–90 cm tall with a waxy bloom, in the deserts of northern Mexico and west Texas. It has an irritant milky sap.
- Bayberry or wax myrtle (Morella species): aromatic shrubs of North American coasts and sandy heaths. In autumn the female bushes carry clusters of small grey, waxy berries close along the twigs.
- Japan wax: berries of East Asian wax and lacquer trees, relatives of poison ivy (see Dangers).
- Crude oil: paraffin wax is in the heavy fraction (Petroleum and Refining); oils that set like jelly in winter are richest. Ozokerite, a mineral wax found in seams in some oilfields, refines to ceresin.
Beeswax
Rendering and cleaning
The basic rendering in water is in Beekeeping. To get clean, bright wax from a mixed lot of comb:
- Soak old dark brood comb in rainwater for 2–3 days. Change the water when it is brown. This takes out honey, pollen and much of the colour.
- Render in water over gentle heat, press the hot mass in a cloth bag between boards, and let the wax set on the water.
- Scrape the soft, dirty layer from the bottom of the cake.
- Clarify. Melt the cake again over water and hold it melted, without stirring, for one to two hours. Wrap the pot in a blanket so it cools slowly. Dirt and water sink. Then pour or ladle the top through felt into the moulds, leaving the bottom layer behind.
Solar wax melter
The solar wax melter melts wax with sunlight alone. It cannot boil over or catch fire, and the sun bleaches the wax a little as it melts.
- Build a wooden box about 60 × 45 cm, 15 cm deep at the front and 25 cm at the back, so the lid slopes toward the midday sun. Paint the inside black and insulate the bottom and sides with 3–5 cm of straw or wool (Insulation and Keeping Buildings Warm or Cool).
- Fit a lid of two panes of glass 1–2 cm apart (Window Glass); two panes get far hotter than one.
- Inside, lay a tinplate or aluminium tray sloping down toward the front at about 15° (Sheet Metal and Rolling).
- At its low end put a strainer of cheesecloth or fine mesh, and under it a pan with a little water in it so the set wax lifts off easily.
- Load comb on the tray and face the box to the sun. On a clear summer day it reaches 70–90 °C and wax runs within an hour.
Good versus bad: a good melter melts a tray of cappings by noon on a sunny day. If wax only softens, the glass is single, the box leaks air, or it faces away from the sun.
Bleaching
Sun bleaching, the old way, gives pure white wax without chemicals.
- Make ribbons: pour melted wax in a thin stream onto a wet wooden roller turning half in cold water, or drip it from a height into cold water.
- Spread the ribbons 2–3 cm deep on linen frames in full sun. Sprinkle with water and turn them every day or two.
- After two to three weeks the outside is white. Re-melt, make ribbons again, and repeat two or three times until it is white right through.
Faster: stir melted wax with 2–5% activated charcoal or bleaching clay at 85–90 °C for an hour and filter hot through felt (Activated Charcoal); or stir it at 90 °C with a few percent of hydrogen peroxide solution, no stronger than about 30 % (Hydrogen Peroxide and Oxygen Bleach), and wash with hot water. White wax is for cosmetics (Toothpaste, Shampoo, Perfume and Cosmetics), ointments (Pharmacy: Tablets, Capsules, Ointments and Inhalers) and fine polish; yellow wax does everything else as well.
Testing beeswax
- Smell and feel: honey smell; warmed in the hand it becomes plastic and kneadable and does not stick to the fingers. A broken face is dull and fine-grained.
- Paraffin added: the wax looks glassy, feels slippery, has little smell, and crumbles when kneaded.
- Tallow added: it feels greasy, smells of fat when warmed, and leaves a grease spot on paper.
- Melting point: put a crumb in a thin glass tube in a water bath with a thermometer. Pure beeswax clears at 62–64 °C. A lower or wider range means it has been mixed with something else.
Plant waxes
Carnauba
- Cut leaves in the dry season, taking only the outer, opened leaves and leaving the central shoot and the youngest leaves on the palm. Unopened young leaves give the palest, best wax. Older leaves give darker wax.
- Dry them in the sun, laid flat in rows, for one to two weeks until they are brittle and the coating flakes.
- Beat them over a cloth in a closed shed, or shred them and shake them in a drum. A grey-white powder falls off.
- Melt the powder in a little hot water, strain through cloth, and let the wax set. It sets as a hard, brittle yellow to grey-brown cake.
The yield is small, a few grams per leaf, so plan on a hundred or more leaves per kilogram. But carnauba is so hard that 10–20% of it in beeswax or paraffin is enough to lift a polish's melting point and shine.
Candelilla
- Pull whole plants by hand in the dry season, leaving roots and some stems so the clump regrows.
- Boil them in a large open pot of water to which a little sulfuric acid has been added, about 2–3 mL per litre of water. The acid helps free the wax from the stems.
- The wax floats up as a brown froth. Skim it into a second pot and let it set.
- Refine: melt it again with a little acid water, let the dirt settle, and pour off the clear wax. Expect about 3–5% of the dry weight of plants as wax.
Bayberry
- Pick the grey berries in autumn, stripping them from the twigs into a basket.
- Boil them in plenty of water for 15–30 minutes, pressing them with a paddle. The wax melts and floats.
- Cool and lift off the green cake. Re-melt it in clean water and strain to clean it.
- Expect about 1 kg of wax from 15 kg of berries. The wax is green, smells of balsam, and is brittle. Blend 1 part bayberry to 1 part beeswax for candles that are hard and fragrant (Lamps and Candles).
Paraffin wax from oil
The Petroleum and Refining chapter separates crude wax from heavy distillate by chilling and pressing. That slack wax still holds 10–30% oil, which makes it soft, greasy and smoky. Refine it as follows:
- Press again, warmer: re-melt, set it in thin cakes, and press them through canvas in a screw press (Oils and Pressing) at about 20–25 °C.
- Sweat. Lay the cakes on wire-mesh trays over drip pans in a closed, heated room. Raise the temperature slowly, about 2 °C an hour, from 25 °C to a few degrees below the wax's melting point, over one to two days. Oil and soft wax drip away, leaving harder scale wax with under 1–2% oil.
- Decolour: stir in 5–10% bleaching clay or charcoal at 90–100 °C and filter hot. For pure white, first stir with 3–5% concentrated sulfuric acid, settle off the black tar, and wash.
- Grade by melting point: what sweats out at lower temperatures is soft wax (48–52 °C) for wraps and blends; what stays is hard wax (56–62 °C) for candles and hot climates.
Microcrystalline wax, from the very heaviest oil residue, needs solvents to separate and is an industrial product. Treat it as a later step. Montan wax, dissolved out of brown coal with hot solvents, is another hard wax for polishes and carbon paper (Coal and Coke).
Things made with wax
Wax block
Store, trade and measure wax as cast blocks of known weight.
- Moulds: tins or wooden boxes wiped with soapy water so the wax releases; 0.5 kg and 1 kg are common sizes.
- Pour beeswax at 70–80 °C, just above melting. Hotter wax cracks and shrinks a deep hollow in the top.
- Cool slowly under a cloth in a warm room, turn out, scrape the bottom face, and stamp the weight and kind.
Hand blocks of 30–50 g: draw thread across one to stiffen it and stop it tangling and rotting (Sewing, Needles and Thread, Leatherwork and Harness-Making); rub one on drawer runners, saws, plane soles, wooden screws and ski soles (Snowshoes, Skis and Sledges). Cobbler's wax is a stiffer blend of pitch, resin and wax for shoe thread (Footwear).
Wax polish
Wax polish feeds and shines wood, floors, leather, stone and iron, leaving a thin skin that water beads on.
- Melt 100 g of beeswax in a tin standing in hot water, with 10–20 g of carnauba or candelilla for a harder shine (a third carnauba for floors).
- Away from any flame, stir in 200–300 g of turpentine: less for a stiff paste, more for a soft one. Pour into lidded tins.
- Use: rub on a thin coat, let the turpentine evaporate for 15–20 minutes, and buff hard with a soft cloth until it no longer smears. Two thin coats beat one thick one.
Cream polish (no turpentine): melt 100 g beeswax; boil 300 mL water with 10 g of borax (Borax and Boric Acid) or 5 g of potash (Lye and Potash); pour the hot water into the wax and stir hard until it cools to a smooth white cream. The alkali makes a little soap from the wax's own acids, and that holds wax and water together. It suits furniture indoors and has no fumes.
Good versus bad: a good polish buffs out in a minute without streaks; a pressed fingertip leaves no mark after buffing. A polish that stays sticky has too little hard wax or too much soft wax or resin.
Shoe polish
Mix by weight 10 parts carnauba, 15 parts beeswax, 75 parts turpentine, and for black 3–5 parts lampblack (Lampblack and Carbon Black). Melt the waxes, take them off the heat, stir in the turpentine and then the black, and pour into small tins. For brown, use burnt umber or another earth pigment (Pigments, Paints and Varnish). Brush it on thinly, let it dry five minutes, and brush or rub to a shine (Footwear, Hides and Leather).
Wax cloth
Wax cloth is cotton filled with a sticky wax blend. It wraps bread, cheese, vegetables and bowls in place of a lid, and keeps food moist without sweating. The heavier waxed canvas for coats and covers is in Raincoats, Oilskins, Umbrellas and Rubber Boots.
- Cut thin, close-woven cotton into squares of 20, 30 and 35 cm, with pinked or hemmed edges (Cotton, Sewing, Needles and Thread).
- Make the blend by weight: 4 parts beeswax, 1 part pine resin, 1 part plant oil (a non-drying oil such as olive; see Oils and Pressing). Melt together over water. The resin makes it cling; the oil keeps it from cracking.
- Lay a square on a tin sheet. Brush or sprinkle about 15–20 g of blend over a 30 cm square.
- Put it in a warm oven at 80–90 °C for 3–5 minutes, or iron it under paper, until the cloth turns evenly dark and wet-looking. Spread any dry spots with the brush.
- Lift it by two corners, wave it for half a minute to set, and hang it to cool.
Use the warmth of your hands to mould it round a bowl or a loaf. Wash in cold water with a little soap, never hot. Re-wax when it stops clinging, after six months to a year. Do not use it for raw meat or fish: it cannot be washed hot enough to be safe.
Modelling wax
For lost-wax casting (Metal Casting, Bronze, Jewellery, Beads and Medals):
- General modelling wax: 4 parts beeswax, 1 part pine resin, ½ part tallow or plant oil. It is soft and workable at hand heat and takes fine detail. Use less tallow in summer and more in winter.
- Carving wax for small precise parts: beeswax with 20–30% carnauba or hard paraffin. It can be filed and turned on a The Lathe.
- Sprue wax: plain paraffin rolled into rods, which melts out fast.
Beeswax and paraffin burn out of a hot mould and leave almost no ash. Resin and fats leave a little, so burn out thoroughly.
Batik and the tjanting
Batik is patterned cloth made by drawing in hot wax, dyeing, and removing the wax. Wherever the wax soaked in, the dye cannot reach.
Making a tjanting:
- Raise a small cup 2.5–3 cm across and 2 cm deep from 0.3–0.5 mm copper sheet (Metal Spinning and Raising, Copper Smelting). Copper holds heat, so the wax stays liquid while you draw.
- Roll a spout of thin copper around a needle or fine wire, 1.5–2 cm long, with a bore of 0.5 mm for fine lines up to 2 mm for broad ones. Fit it into a hole near the bottom of the cup and rivet or braze it (Soldering and Brazing).
- Push a stiff copper tang from the cup into a bamboo or wooden handle 12–15 cm long.
Making batik:
- Wax: about 60% paraffin and 40% beeswax. Paraffin cracks and lets in fine veins of dye (the "crackle" look); beeswax gives clean edges.
- Heat it over a low, steady heat to about 100–120 °C. It is right when a drawn line turns the cloth dark and translucent right through. A pale line sitting on top means too cool; a line that spreads and smokes means too hot.
- Draw on washed, unsized cotton or silk (Cotton, Silk) stretched on a frame. Fill large areas with a brush. Print repeats with a cap, a stamp of copper strips set on edge in a handle.
- Dye in a cold bath such as indigo (Dyes and Mordants); a hot bath melts the wax.
- Repeat: wax over what should keep the first colour, and dye again darker.
- Remove the wax by boiling the cloth in water with a little soda (Soda Ash and Baking Soda). Skim the wax for reuse and iron out the last traces between absorbent paper.
Seals, coatings and insulation
- Jars and bottles: a 3–5 mm layer of paraffin poured on jam, or a cork dipped in wax (Canning and Bottling). Sealing wax for letters is a resin-based blend (Glues and Adhesives).
- Cheese: dip cool, dry, rinded cheeses twice for a second in paraffin or a paraffin–microcrystalline blend at 80–90 °C (Dairy and Cheese).
- Wood and leather: rub warm wax into the end grain of new timber to slow cracking. Make dubbin for boots from 2 parts beeswax, 2 parts tallow and 1 part plant oil.
- Paper: wax paper for wrapping (Sacks, Boxes, Crates and Packaging), match splints dipped in paraffin so they burn (Matches).
- Electrical: paraffin soaks paper for capacitors and seals coils and transformers against damp (The Transformer).
- Writing and recording: wax tablets (Writing and Numbers) and wax cylinders for recording sound (Recording Sound).
How to tell it worked
- Clean wax: even colour right through, no dark bottom layer, burns with a clear flame without spitting.
- Bleached wax: white through a broken block, not only on the surface.
- Paraffin: odourless, leaves no grease spot on paper, and its candles do not smoke.
- Polish, wax cloth, batik: as under each item above.
Note Troubleshooting Wax dark or grey after rendering → heated too hot, melted in an iron or copper pot, or the comb was not soaked first. Re-melt over water in a tin pot; filter through charcoal. Wax full of fine dirt → not held melted long enough to settle; clarify again and pour only the top. Blocks crack → poured too hot or cooled too fast; pour cooler and cover. Paraffin soft and greasy → too much oil left in it; sweat it longer and slower. Polish streaky → applied too thick or buffed too soon; wait for the turpentine to evaporate. Batik lines let dye through → wax too cool; it sat on top instead of soaking in. Or the dye bath was warm. Candelilla wax brown and soft → plant matter left in; refine again with acid water.
Dangers
Danger Wax fires. Wax gives off flammable vapour when it is overheated. Above about 200 °C that vapour can catch from a flame, and hotter still it bursts into flame on its own. Always melt wax over water, never directly over a flame, and never leave it. If melting wax catches fire, cover it with a lid or a damp cloth and take away the heat. Never pour water on burning wax. The water flashes to steam under the wax and throws a ball of burning wax across the room.
- Hot wax burns. Melted wax sticks to skin and keeps burning. Plunge the part straight into cold water. Leave the set wax on the burn and let it come off later (Wound Care and Antiseptics).
- Turpentine vapour catches fire easily and causes headaches. Mix polish away from flames, in a draught. Keep it from children: swallowed, it damages the lungs.
- Japan wax trees and candelilla. The wax tree and lacquer tree belong to the poison-ivy family. Their sap and leaves cause severe, blistering rashes, so wear gloves and long sleeves to harvest the berries. Candelilla and other euphorbias have an irritant milky sap that harms eyes and skin.
- Acids: candelilla and paraffin refining use sulfuric acid (Sulfuric Acid).
- Waxed floors are slippery. Buff them hard and do not over-wax stairs.
What this unlocks
Clean wax gives the best candles, and white wax medical ointments (Pharmacy: Tablets, Capsules, Ointments and Inhalers) and cosmetics (Toothpaste, Shampoo, Perfume and Cosmetics). Modelling wax gives lost-wax castings in Bronze, Jewellery, Beads and Medals and dental work (Dentistry). Polish keeps Furniture, floors (Stairs, Floors and Interior Finishes), Footwear and tools in good order. Batik opens a whole art of patterned cloth (Dyes and Mordants). Paraffin insulates electrical parts and seals food (Canning and Bottling, Dairy and Cheese). It is also a step toward lubricants (Lubricants and Greases) and the light products of the oil refinery (Petroleum and Refining).
How it was first done
Traces of beeswax in the pots of the first farmers of Anatolia and Europe show it in use at least 9,000 years ago. The earliest known lost-wax castings, from Mehrgarh in Pakistan and the Nahal Mishmar hoard in Israel, are more than 5,500 years old. Egyptians used wax in mummification and painted the Fayum portraits (1st–3rd centuries AD) in hot coloured wax. Greek and Roman pupils wrote on wax tablets, and Pliny described "Punic wax", beeswax bleached by boiling in seawater with natron and drying in the sun. Wax-resist dyeing is old in Egypt, India, China and Japan. Javanese batik, drawn with the tjanting, probably reached its classic form by the 1600s–1700s.
English colonists in New England made bayberry candles from the 1600s. Carnauba became an export of north-eastern Brazil in the 1800s and was used in polishes and early gramophone records. Candelilla was gathered commercially in Mexico from the early 1900s. Karl von Reichenbach isolated paraffin from wood tar in 1830, and James Young in Scotland began making paraffin wax and oil from coal and shale around 1850. Paraffin candles soon became the ordinary candle of the world.