Lead

The easiest metal of all to smelt — grey galena gives up its lead in a hot fire. Lead makes pipes, roofs, weights, solder, type and batteries, and it carries silver out of its ores. It is also a slow, silent poison, and this chapter shows how to use it without being harmed.

Difficulty
●●●●●
Time
An afternoon to prove the ore; a day to roast and a day to smelt a batch; an hour to cast sheet
Steps from zero
9 prerequisites →

You need first

Finding and Identifying OresCharcoalBellows

This unlocks

Pipes, Plumbing and AqueductsThe Rechargeable BatteryOptical Glass and Achromatic LensesGold and SilverSoldering and Brazing

Objects made here

ore hearthladlelead sheet
The full path from nothing — 9 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Identifying Ores
  5. Hunting and Trapping
  6. Basic Woodworking
  7. Charcoal
  8. Hides and Leather
  9. Bellows
  10. Lead

Do them roughly in this order. See it on the tech tree →

Why it matters

Lead is soft, heavy and melts at just 327 °C — on a good wood fire. It does not rust away; it bends to any shape by hand; and it is very heavy, more than eleven times the weight of the same volume of water. Those simple facts make it endlessly useful:

  • Weights of every kind: plumb bobs for builders and Surveying and Levelling, net sinkers for Fishing, sounding weights for Navigation, weights for clocks and for balances (see Measurement from Scratch).
  • Roofs and gutters: cast lead sheet seals the joints of a roof against rain for centuries (see Roofs).
  • Pipes: the Latin word for lead, plumbum, gave us "plumber" (but read the warnings in Pipes, Plumbing and Aqueducts before using lead for drinking water).
  • Solder, which joins wires, pipes and tinplate (see Soldering and Brazing), and type metal for Printing.
  • Batteries: the The Rechargeable Battery is the first battery you can recharge.
  • Silver: most silver comes out of lead ore, and molten lead collects silver and gold from other ores. See Gold and Silver.
  • Glass, glazes and paint: lead oxide makes glass sparkle and makes low-temperature glazes, and red lead is a rust-proof paint for iron — all with serious dangers (see below).
  • Shielding from X-Rays, including the treatment beams of Radiotherapy (Overview).

Lead is also poisonous, slowly and invisibly. Every civilisation that used it heavily also poisoned itself with it. You can avoid that if you follow the rules in this chapter.

How it works

The main lead ore is galena, lead sulfide (PbS), which is 87% lead. Two ways turn it into metal:

  1. Roast, then reduce. Heated in air at a dull red heat, galena burns: its sulfur leaves as choking sulfur dioxide gas, and the lead is left as lead oxide. Lead oxide gives up its oxygen to charcoal very easily — at an orange heat, far easier than copper or iron ore — and liquid lead runs out.
  2. Roast–reaction. If you roast only part of the galena, the lead oxide formed reacts with the galena that is left: the oxygen of one and the sulfur of the other leave together as sulfur dioxide, and both give up their lead. This is how the old lead hearths worked. It needs little fuel and moderate heat, about 800–900 °C — bright red.

The second ore, cerussite (lead carbonate), needs no roasting: heated with charcoal it gives lead directly, like malachite gives copper.

Lead is easily lost. Above a bright red heat, lead and its oxide begin to evaporate fast, as poisonous fumes. A lead smelt should be hot, but not too hot — bright red to orange, never yellow-white.

What you need

Item Amount Notes
Galena or cerussite 5–20 kg per batch Hand-picked and crushed to pea size. See Finding and Identifying Ores
Charcoal About equal weight to the ore Or dry hardwood and peat for the hearth
Clay, sand, flat stones For a roasting floor and a small hearth See Finding and Preparing Clay
Bellows One pair See Bellows
Iron scraps (optional) A handful per kg of ore They take up sulfur left in the ore
Iron ladle, iron or clay pot For collecting and casting lead
Moulds Stone, sand or iron. See Metal Casting
Water, soap, a cloth mask For washing hands and damping dust — see Dangers

Where to find it

Look for lead in limestone country, in veins that cut across the rock — often with white calcite, glassy fluorite crystals (purple, green or yellow cubes), quartz, barite (white and surprisingly heavy), and zinc ore. Old mining districts are full of spoil heaps where galena can still be picked up (see Finding and Identifying Ores).

  • Galena is unmistakable once you have held it: bright lead-grey metal shine, breaks into perfect little cubes with mirror-flat faces, very heavy (like a lump of metal), and soft enough to scratch with a copper coin. Its streak is grey-black. Fresh faces tarnish dull grey.
  • Cerussite forms where galena has weathered near the surface: white, grey or colourless, glassy to diamond-bright, and very heavy for a pale mineral. It fizzes in warm vinegar.
  • Anglesite (lead sulfate), often a grey crust round decaying galena, smelts with it.

Tip Prove it on the fire. Put a hazelnut-sized piece of galena in a hollow on a block of charcoal and blow on it with a blowpipe (a hollow reed or a clay tube), or bury it in the hottest part of a campfire under the coals for half an hour. Bright beads of soft metal sweat out. Lead beads scratch with a fingernail, mark paper grey, and flatten under a hammer without cracking. A yellow crust round the spot is lead oxide.

Silver test. Most galena contains some silver — from a trace to more than 1%. Galena with finer, sparkly faces sometimes holds more. Test each new source by cupellation (see Gold and Silver) before you decide what to do with the lead.

Preparing the ore

  1. Hand-pick. Break the vein stuff with a hammer and keep the galena; throw away white calcite and quartz. Zinc ore (brown, resinous sphalerite) and pyrite should also be picked out.
  2. Crush to pieces 5–10 mm across — pea size.
  3. Wash. Galena is so heavy that a few minutes of panning or jigging in a sieve under water leaves it clean (see Finding and Identifying Ores).

Method 1: Roast, then reduce

This is the surest way for a beginner, and it scales from a few hundred grams to tens of kilograms.

1 Roast Crushed galena 3–4 cm deep on embers, dull red (600–700 °C). Stir every 10–15 minutes for 3–6 hours. wind Sulfur dioxidestand upwind Roasting floorstones or fired clay, in the open,far from homes, crops and water 2 Smelt Roasted ore mixed with an equal volume of charcoal, fed on top. Bright red to orange; never yellow-white. Ore + charcoal Tap holeevery 30 min Liquid leadcollects at the bottom
Fig. 1 Lead in two stages. First roast the crushed galena on an open hearth, stirring, at a dull red heat until it stops smoking. Then smelt the roasted ore with charcoal in a bowl hearth; lead runs to the bottom.

Roasting

  1. Build a roasting floor in the open, well away from homes, gardens and water: a flat bed of stones or fired clay about 1 × 1 m, with a low wall on three sides. Light a wood fire on it and let it burn down to a deep bed of embers.
  2. Spread the crushed galena over the embers in a layer no more than 3–4 cm deep.
  3. Keep it at a dull red heat — just visible in shade, about 600–700 °C. Add small wood as needed. Stir it every 10–15 minutes with an iron or green-wood rake, turning the ore over so that every grain meets air.
  4. Watch the smoke. It will give off a sharp, choking smell of burning sulfur (sulfur dioxide). Stand upwind. As the sulfur goes, the shine disappears and the ore turns dull grey, then yellowish-grey.
  5. Do not let it melt. If the ore starts to go soft and sticky, it is too hot: pull the fire back. Melted ore makes hard cakes that roast no further.
  6. Roast for 3–6 hours, until a handful thrown on the fire no longer smells of sulfur. Let it cool; crush any lumps.

Smelting

  1. Use a bowl hearth like the one in Copper Smelting — a clay-lined pit 30 cm across and 20 cm deep, with a low clay collar and a tuyere sloping down into it — but with a tap hole at the bottom on the front side, leading to a small clay-lined dip in the ground outside.
  2. Preheat with charcoal and a gentle blast until the whole hearth glows.
  3. Mix the roasted ore with an equal volume of charcoal in small pieces (1–2 cm). Add a handful of iron scraps per kilogram if you have them. Feed it on top of the burning charcoal, a few handfuls every 5–10 minutes, topping up with charcoal.
  4. Blow moderately. Aim for bright red to orange in front of the tuyere (800–1,000 °C). Do not drive it to yellow; you will see bluish-white fumes and lose lead to the air.
  5. Lead melts and trickles down through the charcoal. Every half hour, open the tap hole with an iron rod and let the lead run into the dip outside, under a sprinkle of charcoal dust. Plug the hole again with clay.
  6. At the end, rake out the grey crust and slag. It still holds lead: crush it, pan it for beads, and smelt it again with more charcoal at a hotter, orange-yellow heat.

A good roast and smelt recovers half to three-quarters of the lead in the ore.

Method 2: The ore hearth (lead in quantity)

For larger amounts, lead smelters used the ore hearth, which uses the roast–reaction and needs no separate roast.

Back wallstone slabs Tuyere15–20 cm up blast Fuel and ore (the "browse")raked out, turned and put back every 10–15 min Lead bath10–12 cm deep Front liplead overflows here Workstonegroove to the pot Poton embers Inside: about 50 cm wide, 40 cm front to back, 30 cm deep
Fig. 2 The lead ore hearth. A bath of molten lead fills the bottom of a stone box; ore and fuel burn on top in the blast; lead runs over the front lip down the workstone into a pot.
  1. Build the hearth: a box of stone slabs or fired clay about 50 cm wide, 40 cm from front to back and 30 cm deep inside. Set the tuyere through the back wall, 15–20 cm above the floor. The front wall is lower (about 15 cm), and in front of it slopes a flat stone — the workstone — with a groove cut down it to a clay or iron pot set in embers.
  2. Start with lead. Melt lead (from Method 1) in the hearth until it fills the bottom 10–12 cm, just below the tuyere. This bath is the heart of the hearth: the burning ore floats on it, and new lead drains into it.
  3. Fuel and ore. Pile glowing charcoal (or dry peat and wood) on the bath and blow. Add washed, crushed galena on top, a few kilograms at a time, mixed with fuel.
  4. Work the browse. Every 10–15 minutes, the smelter lifts the half-smelted crust (the browse) out of the hearth onto the workstone with an iron rake, lets the air reach it, breaks up the lumps, throws aside any glassy grey slag, and pushes it back with fresh fuel and ore. This turning roasts part of the ore so it can react with the rest.
  5. Lead overflows. As new lead forms, the bath rises and runs out over the front lip, along the groove and into the pot. Ladle it into ingot moulds.
  6. Keep the heat bright red, not yellow. Too hot and lead fumes away; too cool and the browse goes stiff.
  7. The slag holds much lead. Smelt it separately with charcoal at a higher heat, as in Method 1.

Working with lead

Casting. Lead is the easiest metal to cast. Melt it in an iron pot over a wood fire and pour at about 400 °C — hot enough that a pine shaving dipped in it chars at once but does not burst into flame. Moulds of stone, iron, sand or even hard dry wood (for one or two pours) all work. See Metal Casting.

Sheet lead. Build a flat table about 2 × 1 m with raised wooden side rails. Fill it with fine, dry sand and smooth it dead flat with a straight board. Make a strike — a board that rides on the side rails with its lower edge set 2–3 mm above the sand. Pour a pot of lead across the top end, and at once push the strike down the table: it spreads the lead into an even sheet the thickness of the gap. Lead sheet 2–3 mm thick makes roof flashings, gutters, tank linings and battery plates.

Pipe. Roll a strip of sheet round a smooth wooden rod, bring the edges together, and seal the seam with solder or molten lead poured along it. Lead pipe bends easily round corners. Joints are made by flaring one end and soldering.

Litharge and red lead. Molten lead with air blowing across it at a bright red heat forms a yellow-orange crust: litharge (lead oxide), the same by-product as in cupellation. Ground and heated gently (about 450–480 °C, a heat just short of any glow) with stirring for many hours, litharge turns bright scarlet: red lead. Red lead mixed with linseed oil is an excellent rust-proof paint for iron (see Pigments, Paints and Varnish); litharge is used in Glass and in low-fire Glazes. Both are powerful poisons; make them only in the open air, and never use lead glazes on pots for food or drink.

How to tell it worked

  • Weight. A lead ingot feels astonishingly heavy for its size.
  • Softness. A fingernail scratches it; a knife cuts it like hard cheese. Fresh cuts are bright blue-white and tarnish dull grey within hours.
  • Marks paper. Rubbed on paper, lead leaves a grey line.
  • Bends without springing back — and without cracking.
  • Purity. Lead with too much antimony or copper is harder and more brittle; lead with silver looks the same — only cupellation tells.

Note Troubleshooting. Ore melted into a hard cake while roasting → too hot, or too thick a layer. Break it up, crush it, and roast again thinner and cooler. Grey, brittle "matte" instead of lead → the ore was not roasted enough; sulfur remained. Roast longer, or add iron scraps to the smelt. Bluish-white smoke pouring off and little lead → too hot. Ease the blast. Lead freezes in the tap hole → open it more often; keep a few hot coals in the collecting dip. Sheet lead uneven or full of holes → the lead was too cool, or the sand not level. Pour hotter and work the strike at once.

Dangers

Danger Lead poisoning is slow, silent and permanent. Lead enters the body as fumes, as dust swallowed from dirty hands, and dissolved in food or drink. It builds up for years. Early signs are tiredness, headaches, irritability, aching joints, constipation and stomach cramps ("lead colic"), and a metallic taste. Later come anaemia (pale skin), a blue-grey line along the gums, weak wrists (the hand droops), kidney damage, infertility and miscarriage. In children, even small amounts permanently damage the growing brain, lowering intelligence and causing behaviour problems. There is no safe level, and no simple cure once it is in the bones.

The rules for working with lead:

  1. Fumes: melt and smelt only in the open air, standing upwind. Keep molten lead below the point where it smokes; bluish-white fumes mean you are poisoning yourself. Never melt lead indoors or in a closed workshop.
  2. Dust: never sand, file or scrape lead dry if you can avoid it. Damp it, and sweep up with wet sawdust, not a dry broom.
  3. Hands: wash with soap and water before eating, drinking or smoking, and before touching children. Do not eat or drink in the lead workshop.
  4. Clothes: keep separate work clothes and wash them apart from the family's.
  5. Children and pregnant women must stay away from lead work, roasting floors, slag heaps and lead dust.
  6. Food and drink: never let acid food or drink — wine, vinegar, fruit juice, pickles — touch lead, lead glaze, lead solder or pewter containing lead. The Romans sweetened wine by boiling it in lead pots, and poisoned themselves.
  7. Water: soft, acid water dissolves lead pipes; hard, limy water coats them with a protective scale. Even so, use clay, wood, iron or copper pipes for drinking water whenever you can (see Pipes, Plumbing and Aqueducts).
  8. Roasting sites stay poisoned. Do not grow food, graze animals or let children play on or downwind of them.

Danger Sulfur dioxide from roasting galena burns the eyes, throat and lungs and can kill in a closed space. Roast in the open, upwind, with nobody downwind.

  • Molten metal and water. As with every metal: dry moulds, dry ground, dry tools.

If someone shows signs of lead poisoning, remove the source first — that is the most important treatment. A diet rich in calcium (milk, cheese, greens) and iron (meat, beans) reduces how much lead the body absorbs.

What this unlocks

Lead and tin make soft solder, the key to joining wire and pipes (Soldering and Brazing). Lead, tin and antimony make type for Printing. Lead plates in Sulfuric Acid make the rechargeable The Rechargeable Battery. Lead is how you get silver by cupellation (Gold and Silver), and how you assay the precious metal in any ore. Sheet and pipe serve Roofs and Pipes, Plumbing and Aqueducts; weights serve the The Mechanical Clock, Surveying and Levelling and Fishing.

How it was first done

Lead is one of the oldest smelted metals, because galena gives up lead in an ordinary fire. Lead beads dating to about 6,500 BC were found at Çatalhöyük in Turkey, and lead objects were made in Mesopotamia and Egypt by the 4th millennium BC — probably first discovered when shiny galena was dropped into a hearth. The search for silver drove much early lead mining: the Athenians' silver mines at Laurion (5th century BC) smelted enormous quantities of lead ore and cupelled out the silver.

The Romans used lead on a scale not seen again until the Industrial Revolution — for water pipes, cisterns, roofs, coffins and cooking — and lead pollution from Roman smelting can still be measured in the ice of Greenland's glaciers. In medieval Britain, lead was smelted in boles: large wood fires built on windy hilltops and ridges, which left place names such as "Bole Hill" across the Peak District. The bellows-blown ore hearth replaced them from the 16th century, and coal-fired reverberatory furnaces followed around 1700. The dangers were known early: the Roman writer Vitruvius warned that water from clay pipes was more wholesome than water from lead pipes.