Part 9 · Health and Medicine
Menstrual Pads, Toilet Paper and Continence Care
How to make washable and throw-away menstrual pads, a rubber menstrual cup, pads and bed protection for people who cannot hold their urine, toilet paper and the older ways of wiping, and bedside urinals — and how to wash, dry and store them so they stay clean and private.
- Difficulty
- ●●●●●
- Time
- An evening to sew a set of pads; a day to make a bed pad; a few days for rubber cups or a batch of soft paper
- Steps from zero
- 9 prerequisites →
This unlocks
—The full path from nothing — 9 steps before this one
- Stone Tools
- Fire
- Finding and Preparing Clay
- Pottery
- Farming from Seed
- Cotton
- Lye and Potash
- Soap
- Personal Hygiene
- Menstrual Pads, Toilet Paper and Continence Care
Do them roughly in this order. See it on the tech tree →
Why it matters
Half of all adults bleed for about five days every month for some forty years. Many people — mothers after hard births, old men and women, people with spinal injuries, dementia or a stroke, children who still wet the bed — cannot always hold their urine. And everyone must clean themselves after the latrine. None of this is talked about much, and all of it decides whether a person can go to school, work, travel and sleep with dignity.
Where there is nothing to use, girls miss a week of school in four, people who leak stop leaving the house, and skin breaks down into sores. A few well-made washable things, a private place to wash them and a sunny line to dry them prevent all of that.
Personal Hygiene gives the basic folded menstrual pad and daily washing. This chapter makes the full kit: better pads, a cup, continence pads and bed protection, toilet paper, and urinals.
How it works
Every product here does one of three jobs:
- Absorb — hold liquid in fine spaces between fibres: washed cotton and linen, wool, sphagnum moss, wood-pulp fluff. Raw cotton is waxy and repels water until boiled with alkali.
- Stop it going further — a backing that liquid cannot pass: tightly woven wool still greasy with lanolin (wool grease), cloth soaked in drying oil or wax, or rubberised cloth.
- Keep the skin dry — a top layer that lets liquid pass quickly down into the absorber but does not hold it against the skin. Brushed cotton (flannel) and wool do this well.
The amounts are small but they matter. A whole period is usually only 30–40 ml of blood (less than 80 ml is normal), mostly on the first two or three days. An adult bladder empties 200–400 ml at a time. So a menstrual pad must hold about a tablespoon of liquid between changes; a continence pad must hold a whole cupful at once, fast, without leaking at the edges.
What you need
| Item | Use | Source |
|---|---|---|
| Soft cotton or linen, best old and worn | Top layers, cores | Cotton, Flax, Hemp and Linen |
| Cotton flannel or terry (looped) towelling | Cores | Spinning and Weaving Cloth |
| Fulled wool cloth | Leak-proof backing | Wool, Felt |
| Linseed oil or beeswax | Waterproof backing cloth | Oils and Pressing, Beekeeping |
| Soft rubber | Cups, rubberised sheeting | Rubber |
| Absorbent cotton | Throw-away pads | The First Aid Kit |
| Paper pulp | Toilet paper, pad fluff | Paper |
| Glazed pottery, glass or tinned metal | Urinals | Pottery, Glass, Tin and Pewter |
| Needle, thread, buttons or tapes | Sewing | Sewing, Needles and Thread, Buttons, Buckles, Hooks and Zips |
Where to find it
Cotton grows in warm, frost-free lands; flax and hemp in cool, damp ones. Old shirts and sheets are the best pad cloth there is. Wool comes from sheep. Sphagnum moss grows in acid bogs in cool, wet country: pale green to reddish cushions that squeeze out like a sponge; dried, it holds many times its weight and was used for wound dressings by the ton in the First World War. Cattail (bulrush) seed-heads, the brown "sausages" on reeds at pond edges, break up into soft fluff in late autumn; kapok fluff comes from the pods of the tall tropical kapok tree. Mullein — tall roadside plant with leaves as soft as flannel — and maize cobs, stripped of grain and dried, are the classic country toilet wipes.
Menstrual pads
The washable pad
A good cloth pad has three layers and wings that fold round the underwear and fasten, so it does not twist or slide.
Sizes (length × width of the core):
| Pad | Length | Core width | Core layers |
|---|---|---|---|
| Light or liner | 16–18 cm | 6 cm | 2 |
| Day | 22–25 cm | 6–7 cm | 4–6 |
| Heavy or night | 28–35 cm, wider at the back | 7–8 cm | 6–8 |
The wings make the pad 16–18 cm across at the middle.
Making one:
- Draw a pattern on paper: a long oval of the right length, with two wings 5 cm deep at the middle. Cut a top and a backing from it, 1 cm larger all round for the seam.
- Cut the core: a long rectangle with rounded ends, the core width wide and 3 cm shorter than the pad, from 4–8 layers of soft old cotton, flannel or terry. Stack them and sew round the edge.
- Lay the core in the middle of the wrong side of the top layer and sew it on with a single line round its edge. Keep it at least 1.5 cm clear of the outer seam line: a thick seam rubs and wicks blood out along the edges.
- Put top and backing right sides together, sew round 1 cm in, leaving a 5 cm gap. Turn right side out through the gap, push out the shape, fold in the gap and topstitch all round 3–4 mm from the edge, closing it.
- On the wings, sew a button and buttonhole, a hook and loop of tape, or a pair of tapes to tie (Buttons, Buckles, Hooks and Zips).
The backing. A plain cotton back works if pads are changed often. For leak protection, use fulled wool (rubbed in lanolin as for nappy covers — see Nappies, Feeding Bottles and Baby Gear), or a cloth made waterproof: rub hot beeswax into tight linen until it stops soaking in and iron it to spread it; or brush on two thin coats of boiled linseed oil, drying each for a week in the air (Linoleum, Oilcloth and Floorcloths). Put the waterproof cloth inside, under a cotton back layer, so it never touches skin.
How many: 8–12 per person, so some are always dry. Change every 4–6 hours, more often on heavy days.
A good pad lies flat after washing, has no thick lumps at the edges, and passes a simple test: a tablespoon (15 ml) of water dripped slowly onto the middle soaks in at once, does not run to the edges, and leaves no damp spot on a dry cloth pressed under the back.
The sanitary belt
Where snug underwear is scarce, use a sanitary belt: a 2 cm cotton tape round the waist, buttoned or tied, with a short tab hanging at the front and back middle. A loop pad — a long pad with a 6–8 cm tape tab at each end — is buttoned or pinned to the tabs.
Throw-away pads
Where washing water is short, make pads to use once:
- The filling. Make absorbent cotton: boil raw cotton or cotton waste in water with washing soda or wood-ash lye for 2–3 hours, rinse well, bleach if you can, dry and fluff it (The First Aid Kit). Or tear dry paper pulp sheets into fluff (Paper); or use dried sphagnum moss, picked clean of twigs and dried in the sun; or cattail or kapok fluff.
- The pad. Lay a flat wad of filling 20 × 7 cm and 1.5–2 cm thick on a strip of thin cotton gauze 30 cm long, fold the gauze round it, and let the ends stick out 5 cm as tabs for a belt. A thin paper or oiled-paper sheet under the filling stops it soaking through.
- Disposal. Wrap in paper or a leaf and burn, or drop down a deep pit latrine (Sanitation and Germs). Never put them in a flush toilet or drain — they block it.
The menstrual cup
A menstrual cup is a small, soft bell of rubber worn inside the vagina. It collects blood instead of absorbing it, holds 20–30 ml, and is emptied, rinsed and put back. One cup lasts a year or more and replaces hundreds of pads. Cups of natural gum rubber have been sold since the 1930s and still are.
Sizes: rim 40–42 mm across for young women who have not given birth; 44–46 mm after childbirth. Body 45–55 mm long, plus a stem of 10–15 mm for grip. Wall about 3 mm thick at the rim, tapering to 2 mm in the body, with a thicker solid base.
Making it (an advanced project): mould it exactly like a baby's teat (Nappies, Feeding Bottles and Baby Gear) — a smooth two-part mould of fired clay or turned hardwood, a central core shaped like the inside of the cup, well-kneaded soft rubber compound, cured buried in hot sand at 130–150 °C for about an hour and a half (Rubber). Before curing, pierce 4–6 holes about 1.5 mm across just under the rim with a greased needle. Trim the flash with sharp scissors and smooth any ridge with fine wet stone. Boil three times in fresh water to wash out sulfur.
A good cup is perfectly smooth inside and out, springs back at once when pinched, has no cracks, bubbles or sticky patches, and does not smell of sulfur after boiling. Fill it with water, pinch the rim shut, and squeeze — no water should come out through the walls.
Using it: wash hands. Fold the cup flat and then in half (a "C"), insert it pointing towards the small of the back, not upwards, and let it spring open. To remove, pinch the base to break the seal and ease it out level. Empty into the latrine, rinse, and reinsert. Empty every 4–8 hours and never leave it in more than 12. Boil it for 5 minutes at the end of each period and store it dry in a cloth bag. Throw it away when it turns sticky, cracked or crumbly.
Warning Anything left inside the vagina can cause infection. Wash hands before inserting; never leave a cup (or a home-made plug of cloth or cotton) in for more than 12 hours. Fever, a sunburn-like rash, vomiting and faintness while using one may be toxic shock syndrome, a rare but deadly bacterial poisoning: remove it at once and seek help. Anyone allergic to latex must not use rubber cups.
Continence care
Help that costs nothing
Before making pads, try what reduces leaking:
- Pelvic floor exercises help most women who leak when they cough, laugh or lift, and many men after prostate problems. Squeeze the muscles you would use to stop passing urine and stop breaking wind, hold for 5–10 seconds, relax for as long; do this 10 times, three times a day. Expect improvement after 6–12 weeks.
- Timed visits: take the person to the latrine or offer a urinal every 2–3 hours by day, and before sleep. Many "incontinent" old people simply cannot get there in time.
- Drink enough — strong, dark urine irritates the bladder; cut down tea, coffee and alcohol in the evening.
- Check for causes: a burning bladder infection, constipation pressing on the bladder, or new diabetes (Chronic Diseases) all cause leaking that can be treated.
- A constant trickle after a hard, long labour may be an obstetric fistula — a hole torn between the birth canal and the bladder or bowel. It can be repaired by a skilled surgeon (Basic Surgery); until then, pads, washing and kindness.
The incontinence pad
An incontinence pad is a larger, thicker version of the menstrual pad, shaped like an hourglass to sit between the legs and held up by snug pants:
- Length 45–60 cm, width 25–30 cm at the ends and 12–14 cm at the narrowest middle.
- Core: 6–10 layers of terry towelling or flannel, or a layer of quilted wool batting, placed a little towards the front for men and in the middle for women.
- Top: brushed cotton or wool, so the skin feels drier.
- Back: fulled wool, or rubberised or oiled cloth inside a cotton layer, as for menstrual pads.
- Stitch through all layers in lines 4–5 cm apart, so the core cannot bunch up when wet.
Test it: lay the pad flat and pour 250 ml of water onto the middle over about ten seconds. No water should run off the edges or come through the back. If it does, add core layers or a wool backing.
The bed pad
A bed pad (underpad) protects the mattress and lets one soiled layer be changed without remaking the bed. It is laid across the middle of the bed under the hips, under or instead of the draw sheet (Nursing the Sick).
- Size: about 60 × 90 cm for a single bed, long enough to tuck in at both sides.
- Layers: a top of cotton flannel; a core of 4–6 layers of old towelling, blanket, or wool batting; a bottom of waterproof cloth (rubberised, oiled or waxed), with the waterproof face down.
- Quilt through all layers in a diamond grid every 10 cm, by hand or on a The Sewing Machine, and bind the edges with tape.
- Make 4–6, so one can always be drying.
Without cloth to spare, a shallow tray of dried sphagnum moss or chopped straw under a cloth, changed daily, was used in hospitals and homes for centuries; burn or compost it after use.
Skin care
Urine and stool left on skin break it down into sores. Change wet pads promptly, wash gently with clean water, pat dry, smooth on a thin barrier of clean animal fat, beeswax salve or zinc ointment, and check hips, buttocks and groin daily for redness (Nursing the Sick).
Toilet paper and its alternatives
Most of the world has always washed rather than wiped: a jug or spouted pot of water, poured with the right hand, the bottom cleaned with the left, then the hands washed with soap. It is cleaner than paper and costs nothing. Keep a water pot in every latrine (Sanitation and Germs, Toilets, Sinks, Baths and Showers).
Where people wipe, they have used soft leaves such as mullein (but know and avoid nettles, poison ivy and anything that itches: Dangerous Plants and Animals), moss, snow, dried maize cobs, smooth stones, and rag squares kept in a lidded pail and washed like nappies. All need hands washed afterwards.
Making toilet paper
Toilet paper is the opposite of writing paper. It must be:
- Very thin — about 15–25 grams per square metre, a quarter of the weight of good writing paper.
- Unsized — no gelatin or starch, so it soaks up water (Paper, step 7: leave it out).
- Soft and crinkled, not smooth and stiff.
- Weak when wet, so it breaks up in water and does not block drains or sewers (Sewers and Wastewater).
Method:
- Pulp. Use the softest fibres you have: cotton or linen rags, old paper, straw or hardwood pulp cooked in lye (Paper). Beat it only lightly — long beating makes paper hard and strong.
- Thin sheets. Make the vat mix twice as dilute as for writing paper, and dip the mould shallowly and fast, for a sheet you can see light through.
- Crêpe. The soft crinkle of toilet tissue comes from scraping the sheet off a hot surface while it is still sticky. Couch the wet sheet straight onto a smooth, oiled-and-wiped hot iron plate or stone over embers (too hot to touch for more than a moment, not hot enough to scorch paper). When it is just dry, scrape it off with a thin, flexible blade held at a steep angle; the sheet crumples into fine folds.
- Or soften by hand. Crumple dry thin sheets into a ball, open them, and rub them gently between the palms several times.
- Cut into squares about 11 × 12 cm and stack in a box or on a nail by the latrine.
Test: put a sheet in a jar of water and shake it ten times. Good toilet paper falls apart into fibres. Paper that stays whole will block a pipe or drain — use it only in a pit latrine.
The urinal
A urinal is a bottle or vessel for passing urine without getting up — for the bedridden, the very old, people after surgery, and anyone on a winter night. It is lighter and easier than a bedpan (Nursing the Sick).
The men's urinal is a bottle of about 1 litre, with:
- a neck 4–5 cm across, angled up at about 45° from the body, with a smooth, thick rolled lip;
- one flat side so it lies on the bed without spilling, and a handle on top;
- marks every 100 ml if you are measuring fluid output (Nursing the Sick).
The women's urinal has a wide oval mouth about 12–15 × 7–8 cm, with a smooth rolled rim and a short spout, on a body of about 1 litre held by a handle. It is placed firmly against the body while sitting or lying on the side.
Making them: throw a closed round body on the wheel; cut a hole in the side and attach a separately thrown neck or mouth while leather-hard, slip-joining and smoothing well; pull a handle; glaze inside and out with a lead-free glaze and fire hard (Pottery, Glazes, Stoneware and Porcelain). A gourd with its neck cut and smoothed works for a man. Tinned or enamelled sheet iron (Sheet Metal and Rolling, Enamel on Metal) and blown glass are lighter and see-through for measuring.
Cleaning: empty into the latrine, rinse, wash with soap and hot water, and once a day soak in strong bleach solution or scald with boiling water (Chlorine and Bleach, Sterilising Instruments and Dressings). A urinal that smells even when clean has a crack or a rough glaze — replace it.
Washing, drying and dignity
Wash all pads as in Personal Hygiene: cold water first (hot water cooks blood into cloth), then hot soapy water, two rinses, and a weekly boil (Laundry and Bleaching Cloth). Shame makes people hide damp pads in dark corners, where they grow mould and germs; hang them in the sun under a thin cover cloth, or on a private line in a walled yard. Store them dry in a clean cloth bag, and carry a spare and a waterproof bag for used ones away from home.
Dignity costs nothing. Give every latrine a door, water and a bin with a lid; give girls and women a private place to wash; tell girls about periods before the first one; and for people who leak, change them promptly, behind a screen, without fuss or comment.
How to tell it worked
- Pads stay in place, do not leak at the edges, and dry in a day in the sun.
- Skin under pads stays pale and unbroken.
- Toilet paper breaks up in the jar test; the latrine drain stays clear.
- Urinals are dry-smelling after washing and do not tip on the bed.
- Girls go to school and women go to work every week of the month.
Note Troubleshooting. Pads leak at the sides → core too narrow or not sewn in, or pad twisted: widen the core, add wings. Leaks through the back → add a wool or waterproof layer. Pads stiff and slow to absorb → soap left in them; rinse more, boil in plain water. Stains won't come out → washed hot first; next time cold first; then dry in strong sun, which bleaches. Cup leaks → wrong size or not fully opened: run a finger round it after inserting. Toilet paper harsh → beaten too long or sized; beat less, crêpe it. Paper won't break up → too thick or too much beating; make it thinner.
Dangers
Danger Toxic shock syndrome can kill within a day. Anyone with a cup, tampon or cloth plug inside who gets a sudden high fever, a red rash, vomiting or diarrhoea, and dizziness must remove it at once and get urgent help.
- Infection from dirty, damp pads — itching, smell and sores. Dry in sun; never reuse an unwashed pad.
- Bedsores from wet beds. Change promptly, turn the person, look at the skin daily (Nursing the Sick).
- Stinging and poisonous leaves. Know your wiping leaves before you use them.
- Lead glazes on urinals and pots leach lead; use lead-free glazes.
- Heavy bleeding — soaking a heavy pad every hour for several hours, clots bigger than a coin, or bleeding after the menopause — is not normal and needs a healer (Examining a Patient).
What this unlocks
Absorbent cotton and pulp fluff lead to wound dressings (The First Aid Kit, Wound Care and Antiseptics); rubber moulding leads to teats and medical tubing (Nappies, Feeding Bottles and Baby Gear, Intravenous Fluids); soft paper leads to tissues and paper towels. Good continence care is half of good nursing (Nursing the Sick, Stretchers, Hospital Beds and Patient Equipment).
How it was first done
Women have always made pads from what was at hand — rags, wool, moss, grass and plant fluff — though the details were rarely written down by the men who wrote history. Sanitary belts and washable towels were sold in Europe and America from the late 1800s. In the First World War, nurses found that Cellucotton, a wood-pulp bandage wadding made in the United States, made excellent pads; from 1920 it was sold as Kotex, the first widely used disposable pad. The menstrual cup was patented several times; the American actress Leona Chalmers patented a rubber one in 1937. In the 2000s an Indian inventor, Arunachalam Muruganantham, built simple machines to press wood-pulp pads cheaply, so village women's groups could make and sell their own.
People in China were using paper for wiping by the sixth century AD — the scholar Yan Zhitui wrote that he would not use paper bearing words from the classics for it — and in 1393 the Ming court ordered 720,000 sheets of toilet paper for its officials. Joseph Gayetty sold packaged "medicated paper" in New York from 1857, and toilet paper on perforated rolls spread from the 1880s and 1890s. Bedside urinals of pottery and pewter are found in households and hospitals across Europe and Asia from at least medieval times.