◆ Rebuild

Part 15 · Knowledge and Science

Optical Glass and Achromatic Lenses

How to melt two kinds of very clear glass — light "crown" and heavy lead "flint" — free of bubbles and streaks, measure how strongly each bends and spreads light, and pair them in a lens that brings all colours to one focus. The achromatic lens makes sharp telescopes, microscopes and cameras possible.

Difficulty
●●●●●
Time
A week per glass melt including slow cooling; a day to measure each glass; two to four weeks to grind and test a doublet
Steps from zero
17 prerequisites →

You need first

GlassLeadLenses

This unlocks

Polarised Light
The full path from nothing — 17 steps before this one
  1. Fire
  2. Cordage and Rope
  3. Stone Tools
  4. Finding and Preparing Clay
  5. Finding and Identifying Ores
  6. Hunting and Trapping
  7. Basic Woodworking
  8. The Kiln
  9. Pottery
  10. Charcoal
  11. Hides and Leather
  12. Lime
  13. Lye and Potash
  14. Glass
  15. Bellows
  16. Lead
  17. Lenses
  18. Optical Glass and Achromatic Lenses

Do them roughly in this order. See it on the tech tree →

Why it matters

A single glass lens has a flaw you cannot polish away: it bends blue light more strongly than red, so the colours come to a focus at different distances. Everything seen through it has coloured fringes and a soft blur, and the stronger and wider the lens, the worse it gets. Early astronomers fought this by making telescopes absurdly long and narrow (see The Telescope); early microscopes were so fringed that many scientists distrusted what they showed (The Microscope).

The cure is to make two different kinds of glass and put a lens of each together, so that the colour error of one cancels the colour error of the other. Such a pair is an achromatic lens (achromatic — "without colour"). It gives you:

It is hard work — the purest glass you have made, cooled more slowly than ever, measured and ground to calculated curves — but it needs only the furnaces and grinding methods you already have.

How it works

Refraction. Light slows down in glass. The refractive index (written n) says how much: ordinary window glass has n ≈ 1.52, meaning light goes 1.52 times slower in it than in air. The higher the index, the more a given curve bends light, and the stronger the lens.

Dispersion. The index is not quite the same for every colour. It is a little higher for blue light than for red, so a prism fans white light out into a rainbow and a lens focuses blue slightly closer than red. The amount of fanning is the dispersion: the index for blue minus the index for red.

Crown and flint. Ordinary soda-lime or potash-lime glass ("crown", after the old crown-shaped window glass) has an index of about 1.51–1.52 and low dispersion. Glass with a lot of lead oxide in it ("flint", because the English first made it from crushed flint) has a higher index, about 1.57–1.65, and its dispersion is roughly twice as large. That difference is the whole secret.

The V-number. Opticians put both properties into one figure, the V-number (also called the Abbe number):

V = (n for yellow − 1) ÷ (n for blue − n for red)

A big V means little colour spreading for the amount of bending. Typical crown: V ≈ 58–64. Typical flint: V ≈ 36–42.

Why two glasses cancel. Take a strong convex lens of crown and a weaker concave lens of flint. The concave flint lens undoes part of the crown's bending — but, because flint spreads colours so much more, it undoes all of the crown's colour error. What is left is a lens that still focuses (more weakly than the crown alone) but brings red and blue to the same point.

Single lens Achromatic doublet Blue focus closer Red focus farther Crown glass one lens white light in every image has coloured fringes Crown Flint (lead) weaker, concave Strong convex crown + weaker concave flint, cemented One focus red and blue meet
Fig. 1 Left: a single lens focuses blue light closer than red, so the image is fringed with colour. Right: a convex crown lens and a weaker concave flint lens together bring red and blue to one focus. The flint undoes all of the crown's colour spreading but only part of its bending.

The rule, for two thin lenses in contact, with powers P (power = 1 ÷ focal length):

P(crown) ÷ V(crown) + P(flint) ÷ V(flint) = 0, and P(crown) + P(flint) = P(whole lens)

Solving these two:

P(crown) = P × V₁ ÷ (V₁ − V₂) P(flint) = −P × V₂ ÷ (V₁ − V₂)

where V₁ is the crown's V-number and V₂ the flint's. The worked example below shows how to use them.

What you need

Item Details
A glass furnace that holds 1,200–1,300 °C for a day See Glass; bellows or a strong draught
Covered crucibles Dense white fireclay, walls 2 cm, with a hood or lid; several
A fireclay stirrer A fired fireclay cylinder 3 cm thick, 15 cm long, on a 1.5 m iron rod
Very pure batch materials Below
Red lead From Lead: litharge heated gently in air until scarlet
An annealing kiln you can seal Or a pit of hot ash big enough to bury the pot
Grinding and polishing kit As for Lenses: tools, grits, rouge, pitch
A board, paper, four pins, a long ruler For measuring refractive index
A salt-coloured flame A spirit lamp or clean charcoal fire with a pinch of salt — pure yellow light
Two thin plates of black glass, or glass painted black behind For the strain test
Pine resin or fir balsam For cementing the lenses

Where to find it

  • Quartz for both glasses: white vein quartz or clear quartz pebbles, heated red-hot and quenched in water so they shatter, then crushed and ground in a stone mortar (Glass). For optical glass the sand must be nearly free of iron: wash it, pick out every dark grain, and soak it a day in dilute Hydrochloric Acid to strip rusty coatings, then rinse until the water tastes of nothing.
  • Potash: purified twice from wood-ash lye, as white as you can make it (Lye and Potash). Recrystallise it: dissolve in hot water, let the dirt settle, pour off the clear liquid and boil it dry.
  • Lime: white limestone or chalk, crushed; avoid stone stained yellow or red.
  • Lead: from galena (heavy, grey, shiny cubes that leave a grey streak), smelted to metal and then turned to red lead (Lead).
  • Manganese ore (pyrolusite — soft, black, stains the fingers) in tiny amounts to cancel a faint green tint (Finding and Identifying Ores).

The recipes

All parts by weight. Grind and mix very thoroughly.

Glass Quartz sand Potash Lime Red lead Saltpetre Expected
Crown 100 35 15 (as crushed limestone 27) — 2 n ≈ 1.51–1.52, V ≈ 57–60
Light flint 100 30 — 65 4 n ≈ 1.57–1.58, V ≈ 41–43
Dense flint 100 25 — 100 5 n ≈ 1.61–1.62, V ≈ 36–38
  • Saltpetre (Saltpeter) keeps the melt "oxidising" — rich in oxygen. Without it, smoke or charcoal dust turns some lead oxide back into metal and the glass goes grey or black. It also helps the bubbles rise.
  • Manganese: add 0.1–0.3 parts only if a test thread looks green. Too much turns the glass pink.
  • The expected values are approximate. Your glass must be measured — every melt differs.
  • Dense flint makes a better doublet (the bigger the gap between the two V-numbers, the gentler the curves), but it is softer, scratches easily, attacks the crucible more and streaks more. Start with crown and light flint.

Step by step: melting glass fit for lenses

Ordinary glass is full of tiny bubbles ("seeds") and of streaks ("cords" or striae) — threads of slightly different composition that bend light differently, like the shimmering of hot air over a road. A few small bubbles in a lens do almost no harm. Streaks ruin it. The method below is the one invented by the Swiss bell-founder Pierre-Louis Guinand around 1800: stir the melt and cool it in the pot.

  1. Prepare the crucible. Use the densest, whitest fireclay you have, with fine grog, walls 2 cm thick. Lead glass eats into clay; a hooded crucible (a pot with a roof and a side mouth) keeps out ash and smoke. Fire it first, alone, to full heat. Preheat it slowly before charging.
  2. Charge in portions. Bring the furnace to yellow heat (about 1,200 °C). Add one third of the batch; wait until it has melted down (30–60 minutes); add the next third, and so on. Fill no more than two-thirds full: lead glass foams.
  3. Fine it. Keep it at the highest heat you can — bright yellow, 1,250 °C or more — for 8–12 hours for crown, 6–8 hours for flint (flint is runnier and gives up its bubbles faster). Skim off any scum. Pull a thread now and then on a hot iron rod: when it shows no white specks and very few bubbles, fining is done.
  4. Stir. Preheat the fireclay stirrer at the furnace mouth for an hour until it glows, then lower it into the melt. Stir slowly in circles that reach the bottom and sides — gently, so you do not whip in new bubbles. Stir for 2–3 hours at full heat, then let the fire fall slowly while you keep stirring, until the glass is as thick as cold honey and the stirrer drags hard. Lift the stirrer out carefully. Heavy lead glass tends to settle into layers; stirring is even more important for flint than for crown.
  5. Cool it in the pot. Close the furnace up with clay, let the fire die, and leave the whole furnace to cool for 5–8 days. Do not open it early.
  6. Break and choose. Break the crucible away. The glass block usually cracks into lumps along its streaks. Grind and roughly polish two opposite faces on each lump and look through it at a distant window frame. Choose lumps where the frame looks perfectly straight and steady as you move the lump about. Reject any with visible threads or wavy patches.
  7. Mould the blanks. Put each chosen lump in a shallow clay dish dusted with fine bone ash or chalk, and heat it slowly to a red-orange heat (about 800 °C) until it slumps into a thick disc. Press it flat with a preheated clay paddle if needed.
  8. Fine-anneal. Hold the disc at the annealing heat — the faint glow you can just see in shade, about 530–550 °C for crown, 430–460 °C for lead flint — for several hours, then seal the kiln and let it cool over 3–5 days. A well-insulated kiln buried in ash does it. This is far slower than ordinary annealing (Glass), because any strain left in a lens makes it focus badly and can crack it in the cold.

How to tell the glass is good

The shadow test for streaks. In a dark room, let sunlight in through a hole 1–2 mm wide in a shutter or card (or put a candle behind such a hole). This is a "point" of light. Hold a polished disc in the beam 3–4 m from the hole and look at its shadow on a white card 1–2 m beyond. Perfect glass casts an even, plain shadow. Streaks show as dark-and-bright wavy lines; bubbles as tiny rings. Streaks across the centre: reject. A few bubbles near the edge: keep.

The strain test. Light reflected off a black glass surface at a slant — meeting the plate at about 33° to its surface (57° from straight on) — is polarised: its waves all vibrate in one direction. Set one black plate so it reflects the bright sky upward at that angle, through your disc, onto a second black plate held crosswise, at the same angle, so that you see the first plate's light almost vanish in it. Turn the second plate until it is darkest. Now well-annealed glass looks uniformly dark; strained glass glows with a light or coloured cross or patches. Re-anneal any strained disc more slowly. Polarised Light explains the principle and better polarisers.

Measuring the glass

The refractive index with pins

Pins 1 and 2 10 cm apart Pins 3 and 4 lined up by eye A D straight-on path Salt flame pure yellow light Eye prism, two faces polished n = sin((A + D) ÷ 2) ÷ sin(A ÷ 2) A = angle of prism · D = least deviation (turn the prism until the pin images stop and turn back)
Fig. 2 Measuring the refractive index of a prism with four pins on a board. Light from the yellow salt flame passes the two pins in front, bends through the prism, and the eye lines up two more pins behind. At the setting where the bending is least, the angles give the index.
  1. Make a prism of each glass: a block about 3 cm high with two flat, polished faces meeting at about 60° (the third face can be left rough). Grind flat faces against a flat stone ground true against two others in turn (Lenses).
  2. Measure the prism's angle A. Lay it on paper on a board, draw round it, and measure the angle between the two polished faces with your protractor — or better, extend the lines 30 cm and measure the gap between them to get the angle from a sine table (Geometry and Trigonometry).
  3. Light it with pure yellow. Behind the board, set a flame coloured strongly yellow with salt — this is the sodium yellow that opticians use as their standard colour.
  4. Push in two pins 10 cm apart in a line pointing at one polished face. Look through the other face, low down at the pins' images. Turn the prism slowly: the images move one way, stop, then move back. Stop the prism where they turn back — the minimum deviation.
  5. Push in two more pins on your side so that all four appear exactly in one line. Remove the prism. Draw the line through the first two pins and the line through the last two, and extend both until they cross. The angle between them is the deviation, D.
  6. Calculate:

n = sin((A + D) ÷ 2) ÷ sin(A ÷ 2)

Example: A = 60.0°, D = 38.6°. (A + D) ÷ 2 = 49.3°; sin 49.3° = 0.7581. A ÷ 2 = 30°; sin 30° = 0.5000. n = 0.7581 ÷ 0.5000 = 1.516 — crown glass.

With lines drawn 30–50 cm long, this gives n to about ±0.003, which is enough.

The dispersion

You need the dispersion, or the V-number, to about one part in twenty. Two ways:

  • With a spectroscope (best — see The Spectroscope). Put each prism on the spectroscope table and measure the minimum deviation, just as above, for three of the dark lines in sunlight: red C, yellow D and blue-green F. Work out n for each and then V = (nD − 1) ÷ (nF − nC). This is exactly how Joseph von Fraunhofer measured his glasses in 1814.
  • By cancelling colour (no spectroscope). Grind a thin wedge of crown, with its two faces at about 8°, and a thin wedge of flint. Put them together, thick end against thin end, and look through them at a white window bar on a dark wall. If the bar still shows a red edge on one side and a blue edge on the other, the flint wedge is too weak or too strong; grind its angle a little and try again until the bar shows no colour at all. Then the dispersions are in the inverse ratio of the wedge angles, and V(crown) ÷ V(flint) = (angle of crown wedge × (n crown − 1)) ÷ (angle of flint wedge × (n flint − 1)). This is how John Dollond found his pairs in 1757. It takes a few days of grinding but no other instrument.

Designing the doublet: a worked example

You want a telescope objective 5 cm across with a focal length of 100 cm (f/20 — a long, forgiving lens for a first attempt). Your measurements: crown n = 1.515, V = 58; flint n = 1.615, V = 37.

  1. Power of the whole lens: P = 1 ÷ 100 cm = 0.0100 per cm.
  2. Power of the crown: 0.0100 × 58 ÷ (58 − 37) = 0.0100 × 58 ÷ 21 = 0.02762. Focal length 36.2 cm, convex.
  3. Power of the flint: −0.0100 × 37 ÷ 21 = −0.01762. Focal length −56.8 cm, concave.
  4. Check: 0.02762 − 0.01762 = 0.0100. ✓

The curves. Make the crown equally convex on both sides. For such a lens, radius R = 2 × (n − 1) × f = 2 × 0.515 × 36.2 = 37.3 cm on each face.

Make the flint's front face fit the crown's back face exactly — the same 37.3 cm radius, but hollow — so the two can be cemented together. Its back face then follows from the lens-maker's rule, 1 ÷ f = (n − 1) × (1 ÷ R₁ − 1 ÷ R₂), counting a surface as negative when it is hollow toward the incoming light. Working it through gives a very shallow hollow of radius about 5.4 m — almost flat.

Surface Radius Shape (light coming from the left)
1. Crown front 37.3 cm Convex
2. Crown back = 3. Flint front 37.3 cm Crown convex / flint concave — they fit
4. Flint back about 540 cm Very slightly concave

Thickness. The depth of a curve across a lens of half-width h is about h² ÷ 2R: here 2.5² ÷ 74.6 = 0.08 cm per face. Make the crown 3 mm thick at the edge and so about 5 mm at the centre; the flint about 2.5 mm at the centre and 3.5 mm at the edge.

Grinding. A beautiful convenience: surfaces 2 and 3 are ground on the same pair of tools — the crown's back in the concave tool, the flint's front on the convex one — so they fit automatically. Surface 1 uses the same concave tool. Only surface 4 needs a new, nearly flat pair. If you cannot make a 5.4 m curve, grind it flat: the lens will still remove more than nine-tenths of the colour (its focal length shortens to about 90 cm), and you can deepen it later.

Grind, polish and centre each lens exactly as in Lenses. The crown always faces the sky (or the object).

Cementing. Clean both surfaces perfectly. Warm both lenses on a warm plate to about 80 °C (too hot to hold for long). Put a drop of clear, strained pine resin or fir balsam on the concave flint surface, lower the crown onto it and press gently, sliding it round to drive out every bubble. Centre the two edges against a straight bar while the resin is soft. Let it cool slowly. Cement fills the thin gap and stops reflections. (Fraunhofer did not cement his large lenses; he left a tiny air gap with three thin foil spacers — also fine.)

How to tell it worked

  • The colour test. Mount the lens in a tube with an eyepiece (The Telescope). Look at a bright star or a distant bright lamp, and move slightly inside and outside focus. A single lens shows a red or blue blob that changes colour on either side of focus. A good achromat shows a white disc with at most a faint purple-violet fringe inside focus and a faint yellow-green one outside — the small leftover colour called the secondary spectrum, which no crown-flint pair removes.
  • Against a window bar at 50 m: a dark bar on a bright sky should have no red or blue edges at all.

Note Troubleshooting. Strong red-and-blue fringes like a single lens → the flint is too weak: its V-number was overestimated. Deepen surface 4 (more hollow) a little and test again. Fringes of reversed colour (blue outside focus where red was before) → overcorrected: the flint is too strong; flatten surface 4. Image soft everywhere but colour-free → bad polish, a streaky blank, or strain; test the blanks again. Star image has a tail on one side → the lenses are not centred on each other; warm the cement and slide them true. Grey or black flint glass → lead reduced to metal; more saltpetre, a cleaner fire, a covered pot. Flint full of fine streaks → stir longer and cool the pot more slowly; choose lumps from the middle of the block. Lens cracked after weeks → strain; fine-anneal more slowly.

Dangers

Danger Lead poisons slowly and surely. Red lead and litharge dust, and the fumes from lead glass at full heat, damage the brain, nerves, kidneys and blood — especially in children and pregnant women. Mix lead batch wet or under a damp cloth, outdoors, with the wind behind you. Wash hands and face before eating; never eat, drink or smoke at the work. Keep children away from the furnace and the batch store, and never let lead glass scraps lie where they play. See Lead.

Danger Never look at the sun through a lens or telescope. It blinds instantly and permanently.

  • Old recipes add arsenic to help bubbles rise. Do not: it is a deadly poison, its fumes rise from the pot, and saltpetre and a long, hot fining do the same job (Arsenic).
  • Molten glass and furnaces: burns, and crucibles that crack and pour out glass at 1,200 °C. Stand in leather and wool, never synthetic cloth, and keep the floor dry — water under molten glass flashes into steam.
  • Silica dust from crushing quartz and grinding: always work wet.
  • Hydrochloric acid for washing sand burns skin and eyes (Hydrochloric Acid).

Going further

  • Microscope objectives: tiny achromatic doublets, 3–10 mm across, ground on small brass tools (The Microscope).
  • Prisms for the The Spectroscope, and for erecting the image in field glasses.
  • Camera lenses of two or more achromatic groups (Photography).
  • Better glasses. In the 1880s Otto Schott found that adding barium, boron and other oxides made glasses with new combinations of index and dispersion. With them, three-lens apochromats remove even the secondary spectrum. Borax in a crown batch is the first step in that direction.

How it was first done

The English lawyer Chester Moor Hall worked out the crown-and-flint lens around 1729–1733 and had a few made, but kept it quiet. In 1757–1758 the London optician John Dollond, using thin wedges of crown and English lead "flint" glass (invented by George Ravenscroft in the 1670s), proved it and patented the achromatic lens; his son Peter built a business on it. Streak-free flint came only in small pieces until the Swiss craftsman Pierre-Louis Guinand found, around 1805, that stirring the melt and cooling it in the pot gave clear blocks. In Bavaria the young Joseph von Fraunhofer combined his method with exact measurement, using the dark lines he discovered in sunlight in 1814. His 24 cm lens for the observatory at Dorpat (1824) was the finest telescope of its day. In 1884 Ernst Abbe, Otto Schott and Carl Zeiss founded the glassworks at Jena that made dozens of new optical glasses — and the V-number is named after Abbe.

Source: content/entries/knowledge/optical-glass.md