◆ Rebuild

Part 1 · Staying Alive

Bow and Arrow

How to make a hunting bow from a single piece of wood — choosing the wood, shaping and tillering it, twisting a bowstring — and arrows with fletching and points; plus the spear-thrower (atlatl), a simpler tool that throws a light spear much harder than an arm alone.

Difficulty
●●●●●
Time
A week to a season to dry the stave; 2–4 days to shape and tiller a bow; an hour or two per arrow; weeks of practice before hunting
Steps from zero
3 prerequisites →

You need first

Cordage and RopeBasic Woodworking

This unlocks

—
The full path from nothing — 3 steps before this one
  1. Cordage and Rope
  2. Stone Tools
  3. Basic Woodworking
  4. Bow and Arrow

Do them roughly in this order. See it on the tech tree →

Note This chapter is about getting food. A bow is a hunting tool. Never point a bow or a spear-thrower, loaded or not, at a person, and never shoot where you cannot see what lies beyond your target.

Why it matters

Traps (Hunting and Trapping) and fishing (Fishing) give a steady supply of small animals. But to take a deer, a goat or a bird on the wing, you need something that strikes from a distance before the animal runs. A hand-thrown spear reaches perhaps 10 metres with any accuracy. A spear-thrower roughly doubles that; a bow sends a light, fast arrow 15–30 metres with enough accuracy to hit an animal's heart. The bow made hunting safer and more successful, freed people to hunt alone and quietly, and spread to almost every continent.

The bow is also a lesson in materials. Making one teaches you how wood behaves under stress — the start of Springs, the bow lathe (The Lathe) and the bow drill (Drills and Boring).

How it works

A bow is a spring. When you draw it, you bend the wooden limbs and store your effort in them; when you let go, the limbs snap straight and pass that energy to the arrow.

Back: stretched Belly: squeezedscrape only here Handlestiff, never bends Tillering stickstring pulled into notches5 cm further each time Limbsbend in matching,smooth arcs Goodeven curve Hingewill break
Fig. 1 The parts of a self bow and how it bends. The back (facing the target) is stretched; the belly (facing you) is squeezed. Tillering removes wood from the belly until both limbs bend in a smooth, even curve.
  • The back of the bow is the side facing away from you, towards the target. When drawn it is stretched (in tension).
  • The belly faces you. When drawn it is squeezed (in compression).
  • Wood breaks in two ways: the back splinters if its fibres are cut or weak, or the belly crushes (you see small wrinkles across it, called "chrysals") if it is too thin or the wood too soft. A good bow is designed so that neither happens.
  • Draw weight is the force needed to pull the string back to full draw, usually measured in kilograms (or pounds). A bow for small game and practice needs about 10–15 kg (20–30 lb); for deer-sized animals, about 18–23 kg (40–50 lb) at a draw of about 70 cm.
  • Draw length is how far you pull the string, from the bow's handle to your fingers at your jaw: about 65–72 cm for most adults. Measure yours: hold a stick against your chest and stretch both arms forward along it; the distance from your chest to your fingertips, minus about 5 cm, is roughly your draw length.

A bow made from a single piece of wood is called a self bow. This chapter makes a flatbow — wide, flat limbs with a rectangular cross-section — because it is the most forgiving design and works with many common woods.

What you need

Item Size or amount Notes
Bow stave 1.8 m long, 5–7 cm wide, straight and knot-free From a straight trunk or sapling 8–15 cm thick
Bowstring fibre Enough for a cord 2 m long, 3 mm thick Sinew, or nettle, dogbane, milkweed, flax, hemp (Cordage and Rope)
Arrow shafts 6–12 straight shoots, 80–90 cm, finger-thick Dogwood, viburnum, hazel, wild rose, cane, reed
Feathers 3 per arrow, 10–13 cm of vane Large flight feathers of goose, turkey, swan, crow or hawk
Points 1 per arrow Stone, bone, antler, or fire-hardened wood (Stone Tools)
Glue and binding — Pine-resin pitch or hide glue; fine sinew (Glues and Adhesives)
Tools — Stone axe and wedges, sharp flakes, scrapers, sandstone, a fire (Basic Woodworking)

Where to find it

Bow woods

Wood Quality Notes
Yew (Taxus) The classic Use the cream sapwood as the back, orange heartwood as the belly. All parts are poisonous except the red fruit flesh: don't eat it, and don't breathe the dust (Dangerous Plants and Animals)
Osage orange (Maclura) Superb Southern and central North America; hard yellow-orange wood
Hickory, black locust Excellent Very tough; forgiving of mistakes
Elm, ash, maple Very good Common in temperate lands; make wide flatbows
Hazel, dogwood, hornbeam, juniper, mulberry, lemonwood Good Hazel makes quick bows from straight shoots
Pine, spruce, willow, poplar, cedar Poor Too weak or brittle except as very wide bows

Choosing a tree: look for a straight trunk or sapling 8–15 cm thick, with no branches, knots, twists or damage for at least 1.8 m. Grain that spirals around the trunk (look at the bark furrows) makes a weak bow. Cut it in late winter, when the sap is down.

Arrow shafts

Straight one-year shoots of dogwood, viburnum (one kind is called "arrowwood"), hazel, wild rose, serviceberry, ocean spray or willow, about finger-thick (8–10 mm) at the base. River cane and giant reed make light, straight shafts; fit a hardwood "foreshaft" into the front end to carry the point. Or split straight-grained wood (ash, birch, pine) into square sticks and round them down. Cut shoots in winter, bundle them tightly so they dry straight, and let them dry for 2–4 weeks.

Step by step: the bow

1. Split and dry the stave

  1. Split the log lengthwise into halves or quarters with wedges (Basic Woodworking). Each piece is a stave. A good stave is straight, at least 5 cm wide on the bark side, and as thick as you can get.
  2. Seal the ends with pitch, fat or wax so they don't crack as they dry.
  3. Remove the bark — for elm, ash, hickory and maple, the surface just under the bark becomes the back of the bow. Do not cut into it. Peel the bark, and scrape off the soft inner bark layer down to the clean, smooth wood beneath. That surface is one unbroken growth ring, and it is what keeps the back from splintering.
  4. Rough out the shape now (step 2), because a thin stave dries far faster than a log.
  5. Dry it indoors, off the ground, away from direct fire heat. Weigh it on a simple balance (Measurement from Scratch) every few days: when it stops getting lighter, it is dry. A roughed-out stave takes about 2–6 weeks; a whole log, a year or more.

Tip Quick bow from a sapling. If you need a bow quickly, a straight hazel, ash or hickory sapling 4–5 cm thick, peeled and roughed out, can be dried in a week beside a warm (not hot) fire. It will be weaker and take more "set" than a seasoned bow, but it will shoot.

2. Lay out and rough out

SEEN FROM THE BACK SEEN FROM THE SIDE Handle 10 cm Limb 5 cm wide tapers to 1.5–2 cm at the tip Nock back: untouched growth ring belly: thinned to shape 170–180 cm tip to tip Widths and thicknesses drawn about twice true scale.
Fig. 2 A flatbow seen from the back and from the side, with a working layout. The handle is stiff and does not bend; the limbs narrow towards the tips.
  1. Mark the centre of the stave. Mark a handle 10 cm long centred there, and fades (where the handle widens into the limbs) 5 cm above and below it.
  2. Draw the outline on the back: limbs 5 cm wide from the fades to about halfway out, then tapering evenly to 1.5–2 cm at the tips. Total length, tip to tip, about 170–180 cm for a 70 cm draw — longer is safer; a short bow breaks more easily.
  3. Cut away the sides to the outline with axe and flakes.
  4. Thin from the belly only. Remove wood from the belly side until the limbs are about 2 cm thick at the fades, tapering to about 1.2 cm at the tips. The handle stays thicker (3–4 cm) and stiff. Never touch the back.
  5. Cut the nocks: at each tip, cut a notch on each side, angled towards the handle at 45°, about 5 mm deep, with rounded edges so it won't cut the string.

3. Tiller it

Tillering means shaping the bow, a little at a time, until both limbs bend in a smooth, even curve. It is the most important and the most patient part of the job.

  1. Floor tiller. Put one tip on the ground, hold the other tip, and press gently on the handle. Watch how each limb bends. It will be stiff — that is right.
  2. Make a tillering stick: a board or straight pole about 90 cm long with a notch at the top to hold the bow's handle, and notches every 5 cm down its length for the string.
  3. Use a long string at first (a tillering string, longer than the bow), so the bow can be flexed only a little.
  4. Pull the string into the first notch, perhaps 10–15 cm. Step back and look at the curve against a straight background (the edge of a wall, a straight pole).
    • Any part of a limb that stays straight (stiff) gets wood scraped off its belly.
    • Any part that bends more than the rest (a "hinge") is weak: don't touch it; take wood from the stiff parts around it instead.
  5. Exercise the bow 20–30 times at the new draw before you look again. Wood settles.
  6. Pull a little further each time — 5 cm more — scrape, exercise, look. Both limbs should bend into the same smooth arc, the upper limb very slightly stiffer than the lower.
  7. Brace it. Once it bends to about 40 cm, fit the real string at brace height — about 15 cm from the handle to the string, a fist with the thumb stuck up. Continue tillering at brace.
  8. Check the weight as you near full draw. Hang the bow by its handle from a beam, hang a bark bucket or skin bag from the string, and pour in water until the string reaches full draw. Each litre of water weighs 1 kg. Stop scraping when it reaches your target weight at full draw.
  9. Never pull past your draw length, and never draw beyond the weight you have measured. Most bows break at this stage, from impatience.

4. Finish

  • Smooth the bow with sandstone, then horsetail stems or a scraper.
  • Rub in fat, oil or beeswax and warm it in, to slow the wood taking up and losing moisture.
  • Wrap the handle with leather or cord for grip.
  • Expect a little "set" — the bow stays slightly bent towards the belly after use. A few centimetres is normal.
  • Unstring it whenever you aren't using it. Keep it dry.

Step by step: the bowstring

  1. Sinew: dry tendons from the legs or back (Cordage and Rope), pound them until they separate into fluffy fibres, and twist them into a two-ply reverse-wrapped cord about 3 mm thick. Sinew strings are strong but stretch and weaken when damp; keep them waxed and dry.
  2. Plant fibre: dogbane, milkweed, nettle, flax or hemp, twisted the same way, three strands thick or two thick plies. More reliable in wet weather.
  3. Strength: a string should be at least four times as strong as the bow's draw weight. Test it: hang a weight on a length of the same cord. If in doubt, make it thicker.
  4. Make a loop at one end — while twisting, fold the end back on itself for 8–10 cm and twist it in, making a permanent eye that slips over one nock.
  5. Tie the other end to the second nock with a timber hitch, adjusting the length until the brace height is about 15 cm. The finished string is roughly 8–10 cm shorter than the bow's length from nock to nock.
  6. Wax it with beeswax, or a mix of resin and fat.
  7. Wrap the middle (where the arrow sits and your fingers pull) with fine thread for 10 cm to protect it.
  8. Always carry a spare.

Step by step: arrows

END VIEW cock featherat right anglesto the nock Three feathers10–13 cm, same wing, 120° apart Shaft Pointglued with pitch, bound with sinew Nock5–6 mm slot 75–80 cm: your draw length + 5–8 cm8–10 mm thick
Fig. 3 The parts of an arrow. A straight shaft about 75–80 cm long, a nock slot for the string, three feathers glued and bound near the back, and a point bound into a slot at the front with sinew and pitch.
  1. Peel the dried shoots and scrape off knots.
  2. Straighten: warm each bend over hot coals (not flame), turning it, until it is too hot to hold comfortably. Bend it slightly past straight, hold it until it cools (a minute or so), and sight down the shaft to check. Repeat for each bend. A piece of bone or antler with a hole drilled through it makes a good lever for straightening. Two grooved blocks of sandstone rubbed along the shaft smooth it.
  3. Length: about your draw length plus 5–8 cm — usually 75–80 cm. Cut to length.
  4. Match the set. Arrows for one bow should be the same weight and stiffness. Flex each one over your knee and weigh them on a balance; sort out those that differ much. Heavier bows need stiffer arrows.
  5. Nock: cut a slot 5–6 mm deep in the back end, just wide enough for the string to snap into. Wrap a few turns of sinew just below it so it won't split.
  6. Fletching: take large wing feathers, all from the same wing of one kind of bird (so they curve the same way). Split each down the middle of its quill with a sharp flake and scrape the quill flat. Trim three pieces 10–13 cm long. Glue them on 120° apart, about 3 cm in front of the nock, with one feather (the "cock feather") at right angles to the nock slot. Bind the front and back ends of each quill with fine wet sinew, which shrinks and glues itself as it dries. Trim the feathers to about 1–1.5 cm high by singeing them gently against a hot stone or cutting them on wood with a flake.
  7. Point: cut a slot 1.5–2 cm deep in the front end, fit the point's tang (its base), glue it with hot pitch, and bind it tightly with sinew (Stone Tools). For birds and small animals, a blunt point — a knob of hardwood, or the shaft left thick and rounded — stuns rather than pierces, and doesn't fly as far when it misses. For practice, fire-harden a sharpened wooden tip.
  8. Balance: an arrow flies best when its balance point is a little in front of the middle — the point is the heaviest part.

The spear-thrower (atlatl)

The spear-thrower — called atlatl in Mexico and woomera in Australia — is much simpler to make than a bow, and was used for tens of thousands of years before bows. It is a stick that makes your arm longer, so the light spear (the dart) leaves your hand far faster.

Spurhook at the back Thrower50–60 cm, forearm and hand Dart1.5–2 m, springy, fletched grip both lightly CLOSE UP spur fits a hollow in the dart end THE THROW the thrower is anextra joint: its tipmoves much faster
Fig. 4 A spear-thrower and dart. The hook at the back of the thrower sits in a small hollow in the end of the dart. The throw is like throwing a ball overhand, and the thrower adds an extra joint to your arm.
  1. The thrower: a straight, stiff piece of hardwood 50–60 cm long (about the length of your forearm and hand together), 3–4 cm wide and 1–2 cm thick. At the back end, carve a spur — a small upward hook or peg, 1–2 cm high — or lash on a pointed piece of antler. At the front, shape a grip, or lash on two finger loops of leather.
  2. The dart: a straight, slightly springy shaft 1.5–2 m long and 1–1.5 cm thick, of cane, dogwood, ash or other straight wood. Cut a small cup-shaped hollow in the back end for the spur to sit in. Fletch it with two or three long feathers near the back, as for an arrow but larger (15–20 cm). Fit a sharp point of stone, bone or fire-hardened wood.
  3. Throwing: hold the thrower with the dart lying along it, the spur in the dart's hollow, and the dart held loosely by your fingertips near the front. Raise it beside your head, pointing at the target. Step forward and throw with a smooth, overhand motion like throwing a ball, snapping your wrist at the end. The dart slips off the spur and flies.
  4. Practice: start at 10 m against a bundle of grass. With practice, most people hit an animal-sized target reliably at 15–25 m.

The spear-thrower takes an afternoon to make. Its darts are heavier than arrows and hit hard, but it is harder to throw from cover or kneeling, and you need more open space to throw.

How to tell it worked

  • The bow draws smoothly to full draw without creaking, both limbs bend into matching curves, and the string is centred along the limbs. After 50 shots it has taken no more than a few centimetres of set, and there are no wrinkles across the belly or lifted splinters on the back.
  • The arrows fly point-first without wobbling and land close together. Shoot all your arrows at the same spot from 10 m; any that land well away from the group have a fault (bent, heavier, wrong stiffness, a loose feather).
  • You can put five arrows out of five into a target the size of your hand at 15 m. Only then are you ready to hunt.

Note Troubleshooting. One limb bends more than the other → scrape the belly of the stiffer limb only, a little at a time. A sharp bend in one spot (hinge) → stop working that spot; take wood from the stiff areas either side. A bad hinge usually ends in a break. Wrinkles across the belly → the belly is crushing; the bow is too thin or too short for the wood. Make the next one wider or longer. Splinter lifting on the back → the back ring was cut or damaged. Glue and wrap it with sinew, or start again. Arrows fly sideways or tail-first → feathers on the wrong side, mixed wings, or the arrow is too stiff or too weak for the bow. Make a matched set. String slips off the nock → deepen the nocks or tighten the string loop. Darts wobble off the atlatl → the dart is too stiff or too floppy, or you're pushing instead of throwing; use a slightly more flexible shaft and a smooth, fast throw.

Hunting with a bow

  • Get close. A bow made this way is accurate at 10–20 m, sometimes 25 m. Most of hunting is the stalk: moving slowly from cover to cover, downwind of the animal (Hunting and Trapping), freezing whenever it looks up.
  • Ambush: wait by a trail, a feeding place or water at dawn or dusk, hidden, with an arrow ready.
  • Aim for the heart and lungs — just behind the front leg, a third of the way up the body, when the animal stands side-on or angled slightly away. A shot here kills in seconds to a minute; a shot in the belly or leg means a long, cruel chase.
  • Wait before following. After a good hit, wait 20–30 minutes before following the blood trail quietly; a frightened, wounded animal runs much further. Then gut it at once (Hunting and Trapping, Butchery and Meat).
  • Don't shoot at animals that are moving fast, too far away, or facing you.
  • Birds and small game: blunt points, close range.

Dangers

Danger Bows and darts can kill a person. Never point one at anyone, even as a joke and even without an arrow. Never shoot where you cannot see beyond the target, upwards into the air, or towards houses, paths or the edge of thick cover where someone might be. Keep arrows pointed at the ground when walking with an arrow on the string. Make sure everyone in a hunting group knows where the others are.

  • Breaking bows. A bow breaking at full draw throws splinters towards your face. Protect your eyes while tillering, and never draw past full draw or "dry fire" (release the string without an arrow — the energy goes into the bow and can break it).
  • The string slap. The string hits the inside of your bow arm; wear a leather guard (a bracer) on the forearm, and keep the elbow slightly turned out.
  • Yew is poisonous. Wash hands after working it, don't breathe the dust, and keep children and animals away from the leaves and seeds.
  • Ricochets. Arrows glance off stones and frozen ground. Shoot into earth or a grass bundle, not at rocks.
  • Wounded large animals can turn on you. Approach carefully and from behind (Dangerous Plants and Animals).

What this unlocks

A bow lets you hunt larger game and birds, giving meat, fat, hides and sinew for Hides and Leather and Cordage and Rope, and feathers and bone for more arrows. The skills of reading wood — tension, compression, seasoning — go into tool handles, Springs, the The Lathe and the bow drill (Fire, Drills and Boring). Points of copper, bronze and iron come later with Copper Smelting, Bronze and Blacksmithing. Eventually, keeping animals (Keeping Animals) replaces most hunting.

How it was first done

The spear-thrower is older than the bow in most places. Carved antler hooks from spear-throwers are known from about 17,000–18,000 years ago in France, and spear-throwers may be much older. Bows are harder to trace because wood rots: small stone points with damage and residues that suggest arrows have been found at Sibudu Cave in South Africa dating to around 60,000 years ago, and in Mandrin Cave in France at about 54,000 years ago, though how they were used is still debated. The oldest surviving bows are about 9,000 years old: elm flatbows from Holmegaard in Denmark, wide and flat — very like the bow in this chapter. The 5,300-year-old man found frozen in the Alps (called Ötzi) carried an unfinished yew longbow 1.82 m long and a hide quiver of arrows with flint points and feathers glued and bound with birch tar and fibre. The bow reached Arctic North America about 5,000 years ago and spread across most of the rest of the Americas between about 2,000 and 1,000 years ago. It was never taken up in Australia, where the woomera spear-thrower remained the hunter's tool.

Source: content/entries/survival/bow-and-arrow.md